| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.24 g/cc | 0.0448 lb/in³ | |
| 1.40 g/cc | 0.0506 lb/in³ | DAM; ISO 1183 | |
| Water Absorption | 2.0 % @Thickness 2.00 mm |
2.0 % @Thickness 0.0787 in |
DAM; Sim. to ISO 62 |
| Viscosity | 63230 cP @Shear Rate 5000 1/s, Temperature 280 °C |
63230 cP @Shear Rate 5000 1/s, Temperature 536 °F |
ISO 11403-1 -2 |
| 75340 cP @Shear Rate 5000 1/s, Temperature 270 °C |
75340 cP @Shear Rate 5000 1/s, Temperature 518 °F |
ISO 11403-1 -2 | |
| 90990 cP @Shear Rate 5000 1/s, Temperature 260 °C |
90990 cP @Shear Rate 5000 1/s, Temperature 500 °F |
ISO 11403-1 -2 | |
| 191300 cP @Shear Rate 500 1/s, Temperature 280 °C |
191300 cP @Shear Rate 500 1/s, Temperature 536 °F |
ISO 11403-1 -2 | |
| 238600 cP @Shear Rate 500 1/s, Temperature 270 °C |
238600 cP @Shear Rate 500 1/s, Temperature 518 °F |
ISO 11403-1 -2 | |
| 299100 cP @Shear Rate 500 1/s, Temperature 260 °C |
299100 cP @Shear Rate 500 1/s, Temperature 500 °F |
ISO 11403-1 -2 | |
| Linear Mold Shrinkage, Flow | 0.0020 cm/cm | 0.0020 in/in | DAM; ISO 294-4 2577 |
| Linear Mold Shrinkage, Transverse | 0.0070 cm/cm | 0.0070 in/in | DAM; ISO 294-4 2577 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 120 MPa | 17400 psi | 50%RH; ISO 527-1/-2 |
| 200 MPa | 29000 psi | DAM; ISO 527-1/-2 | |
| Tensile Stress | 8.71 MPa @Strain 0.230 %, Temperature 150 °C |
1260 psi @Strain 0.230 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 |
| 11.56 MPa @Strain 0.230 %, Temperature 90.0 °C |
1677 psi @Strain 0.230 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 12.2 MPa @Strain 0.340 %, Temperature 180 °C |
1770 psi @Strain 0.340 %, Temperature 356 °F |
DAM; ISO 11403-1 -2 | |
| 14.68 MPa @Strain 0.230 %, Temperature 40.0 °C |
2129 psi @Strain 0.230 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 16.28 MPa @Strain 0.220 %, Temperature 23.0 °C |
2361 psi @Strain 0.220 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 17.71 MPa @Strain 0.420 %, Temperature 150 °C |
2569 psi @Strain 0.420 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 23.12 MPa @Strain 0.460 %, Temperature 90.0 °C |
3353 psi @Strain 0.460 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 26.72 MPa @Strain 0.980 %, Temperature 150 °C |
3875 psi @Strain 0.980 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 30.38 MPa @Strain 1.43 %, Temperature 180 °C |
4406 psi @Strain 1.43 %, Temperature 356 °F |
DAM; ISO 11403-1 -2 | |
| 33.64 MPa @Strain 0.330 %, Temperature 0.000 °C |
4879 psi @Strain 0.330 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 35.53 MPa @Strain 0.370 %, Temperature 40.0 °C |
5153 psi @Strain 0.370 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 37.14 MPa @Strain 1.06 %, Temperature 90.0 °C |
5387 psi @Strain 1.06 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 37.88 MPa @Strain 1.93 %, Temperature 150 °C |
5494 psi @Strain 1.93 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 39.58 MPa @Strain 2.60 %, Temperature 180 °C |
5741 psi @Strain 2.60 %, Temperature 356 °F |
DAM; ISO 11403-1 -2 | |
| 41.33 MPa @Strain 1.43 %, Temperature 150 °C |
5994 psi @Strain 1.43 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 42.83 MPa @Strain 0.850 %, Temperature 40.0 °C |
6212 psi @Strain 0.850 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 45.1 MPa @Strain 2.91 %, Temperature 150 °C |
6540 psi @Strain 2.91 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 45.77 MPa @Strain 3.76 %, Temperature 180 °C |
6638 psi @Strain 3.76 %, Temperature 356 °F |
DAM; ISO 11403-1 -2 | |
| 45.92 MPa @Strain 0.760 %, Temperature 23.0 °C |
6660 psi @Strain 0.760 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 52.64 MPa @Strain 1.93 %, Temperature 90.0 °C |
7635 psi @Strain 1.93 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 53.99 MPa @Strain 1.37 %, Temperature 90.0 °C |
7831 psi @Strain 1.37 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 54.69 MPa @Strain 2.57 %, Temperature 150 °C |
7932 psi @Strain 2.57 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 63.52 MPa @Strain 3.75 %, Temperature 150 °C |
9213 psi @Strain 3.75 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 63.66 MPa @Strain 2.84 %, Temperature 90.0 °C |
9233 psi @Strain 2.84 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 63.75 MPa @Strain 1.53 %, Temperature 40.0 °C |
9246 psi @Strain 1.53 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 69.79 MPa @Strain 1.38 %, Temperature 23.0 °C |
10120 psi @Strain 1.38 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 70.99 MPa @Strain 0.560 %, Temperature -20.0 °C |
10300 psi @Strain 0.560 %, Temperature -4.00 °F |
DAM; ISO 11403-1 -2 | |
| 73.26 MPa @Strain 0.650 %, Temperature -20.0 °C |
10630 psi @Strain 0.650 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |
| 74.02 MPa @Strain 2.36 %, Temperature 90.0 °C |
10740 psi @Strain 2.36 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 74.79 MPa @Strain 0.840 %, Temperature 40.0 °C |
10850 psi @Strain 0.840 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 75.42 MPa @Strain 0.830 %, Temperature 0.000 °C |
10940 psi @Strain 0.830 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 76.34 MPa @Strain 0.670 %, Temperature 23.0 °C |
11070 psi @Strain 0.670 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 81.87 MPa @Strain 2.38 %, Temperature 40.0 °C |
11870 psi @Strain 2.38 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 83.18 MPa @Strain 0.730 %, Temperature 0.000 °C |
12060 psi @Strain 0.730 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 88.65 MPa @Strain 3.49 %, Temperature 90.0 °C |
12860 psi @Strain 3.49 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 90.74 MPa @Strain 2.15 %, Temperature 23.0 °C |
13160 psi @Strain 2.15 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 104.32 MPa @Strain 1.31 %, Temperature 0.000 °C |
15130 psi @Strain 1.31 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 104.43 MPa @Strain 1.32 %, Temperature 40.0 °C |
15146 psi @Strain 1.32 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 110.27 MPa @Strain 1.04 %, Temperature -20.0 °C |
15993 psi @Strain 1.04 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |
| 112.55 MPa @Strain 1.05 %, Temperature 23.0 °C |
16324 psi @Strain 1.05 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 121.66 MPa @Strain 5.75 %, Temperature 23.0 °C |
17645 psi @Strain 5.75 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 121.88 MPa @Strain 1.13 %, Temperature 0.000 °C |
17677 psi @Strain 1.13 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 129.33 MPa @Strain 1.88 %, Temperature 0.000 °C |
18758 psi @Strain 1.88 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 129.58 MPa @Strain 1.90 %, Temperature 40.0 °C |
18794 psi @Strain 1.90 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 142.92 MPa @Strain 1.44 %, Temperature 23.0 °C |
20729 psi @Strain 1.44 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 143.73 MPa @Strain 1.49 %, Temperature -20.0 °C |
20846 psi @Strain 1.49 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |
| 156.52 MPa @Strain 1.55 %, Temperature 0.000 °C |
22701 psi @Strain 1.55 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 159.95 MPa @Strain 1.46 %, Temperature -20.0 °C |
23199 psi @Strain 1.46 %, Temperature -4.00 °F |
DAM; ISO 11403-1 -2 | |
| 171.1 MPa @Strain 1.94 %, Temperature 23.0 °C |
24820 psi @Strain 1.94 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 174.04 MPa @Strain 2.02 %, Temperature -20.0 °C |
25242 psi @Strain 2.02 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |
| 188.32 MPa @Strain 2.05 %, Temperature 0.000 °C |
27314 psi @Strain 2.05 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 |