| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 8.25 g/cc | 0.298 lb/in³ |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Brinell | 318 @Temperature 760 °C |
318 @Temperature 1400 °F |
Converted from Rockwell C hardness (aged) |
| Hardness, Knoop | 343 @Temperature 760 °C |
343 @Temperature 1400 °F |
Converted from Rockwell C hardness (aged) |
| Hardness, Rockwell B | 97 @Temperature 760 °C |
97 @Temperature 1400 °F |
annealed |
| Hardness, Rockwell C | 34 @Temperature 760 °C |
34 @Temperature 1400 °F |
aged |
| Hardness, Vickers | 332 @Temperature 760 °C |
332 @Temperature 1400 °F |
Converted from Rockwell C hardness (aged) |
| Tensile Strength, Ultimate | 900 MPa @Temperature 760 °C |
131000 psi @Temperature 1400 °F |
|
| Tensile Strength, Yield | 702 MPa @Strain 0.200 %, Temperature 760 °C |
102000 psi @Strain 0.200 %, Temperature 1400 °F |
|
| Elongation at Break | 12 % @Temperature 760 °C |
12 % @Temperature 1400 °F |
in 50.8 mm |
| Modulus of Elasticity | 150 GPa @Temperature 927 °C |
21800 ksi @Temperature 1700 °F |
|
| 160 GPa @Temperature 871 °C |
23200 ksi @Temperature 1600 °F |
||
| 163 GPa @Temperature 843 °C |
23600 ksi @Temperature 1550 °F |
||
| 166 GPa @Temperature 816 °C |
24100 ksi @Temperature 1500 °F |
||
| 171 GPa @Temperature 760 °C |
24800 ksi @Temperature 1400 °F |
||
| 178 GPa @Temperature 677 °C |
25800 ksi @Temperature 1250 °F |
||
| 179 GPa @Temperature 649 °C |
26000 ksi @Temperature 1200 °F |
||
| 182 GPa @Temperature 593 °C |
26400 ksi @Temperature 1100 °F |
||
| 188 GPa @Temperature 538 °C |
27300 ksi @Temperature 1000 °F |
||
| 190 GPa @Temperature 482 °C |
27600 ksi @Temperature 900 °F |
||
| 198 GPa @Temperature 371 °C |
28700 ksi @Temperature 700 °F |
||
| 204 GPa @Temperature 260 °C |
29600 ksi @Temperature 500 °F |
||
| 213 GPa @Temperature 149 °C |
30900 ksi @Temperature 300 °F |
||
| 218 GPa @Temperature 21.0 °C |
31600 ksi @Temperature 69.8 °F |
||
| Poissons Ratio | 0.31 @Temperature 149 °C |
0.31 @Temperature 300 °F |
|
| 0.31 @Temperature 27.0 °C |
0.31 @Temperature 80.6 °F |
||
| 0.32 @Temperature 482 °C |
0.32 @Temperature 900 °F |
||
| 0.32 @Temperature 371 °C |
0.32 @Temperature 700 °F |
||
| 0.32 @Temperature 260 °C |
0.32 @Temperature 500 °F |
||
| 0.33 @Temperature 649 °C |
0.33 @Temperature 1200 °F |
||
| 0.33 @Temperature 760 °C |
0.33 @Temperature 1400 °F |
||
| 0.33 @Temperature 677 °C |
0.33 @Temperature 1250 °F |
||
| 0.34 @Temperature 843 °C |
0.34 @Temperature 1550 °F |
||
| 0.35 @Temperature 927 °C |
0.35 @Temperature 1700 °F |
||
| Shear Modulus | 55.0 GPa @Temperature 927 °C |
7980 ksi @Temperature 1700 °F |
|
| 61.0 GPa @Temperature 843 °C |
8850 ksi @Temperature 1550 °F |
||
| 64.0 GPa @Temperature 760 °C |
9280 ksi @Temperature 1400 °F |
||
| 67.0 GPa @Temperature 677 °C |
9720 ksi @Temperature 1250 °F |
||
| 69.0 GPa @Temperature 593 °C |
10000 ksi @Temperature 1100 °F |
||
| 72.0 GPa @Temperature 482 °C |
10400 ksi @Temperature 900 °F |
||
| 75.0 GPa @Temperature 371 °C |
10900 ksi @Temperature 700 °F |
||
| 77.0 GPa @Temperature 260 °C |
11200 ksi @Temperature 500 °F |
||
| 81.0 GPa @Temperature 149 °C |
11700 ksi @Temperature 300 °F |
||
| 83.0 GPa @Temperature 27.0 °C |
12000 ksi @Temperature 80.6 °F |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear | 13.5 µm/m-°C @Temperature 21.0 - 538 °C |
7.50 µin/in-°F @Temperature 69.8 - 1000 °F |
|
| 14.0 µm/m-°C @Temperature 21.0 - 649 °C |
7.78 µin/in-°F @Temperature 69.8 - 1200 °F |
||
| 14.8 µm/m-°C @Temperature 21.0 - 760 °C |
8.22 µin/in-°F @Temperature 69.8 - 1400 °F |
||
| 15.2 µm/m-°C @Temperature 21.0 - 871 °C |
8.44 µin/in-°F @Temperature 69.8 - 1600 °F |
||
| 16.3 µm/m-°C @Temperature 21.0 - 927 °C |
9.06 µin/in-°F @Temperature 69.8 - 1700 °F |
||
| 16.8 µm/m-°C @Temperature 21.0 - 982 °C |
9.33 µin/in-°F @Temperature 69.8 - 1800 °F |
||
| Specific Heat Capacity | 0.452 J/g-°C @Temperature 27.0 °C |
0.108 BTU/lb-°F @Temperature 80.6 °F |
|
| Thermal Conductivity | 11.5 W/m-K @Temperature 149 °C |
79.8 BTU-in/hr-ft²-°F @Temperature 300 °F |
|
| 12.5 W/m-K @Temperature 204 °C |
86.8 BTU-in/hr-ft²-°F @Temperature 399 °F |
||
| 13.6 W/m-K @Temperature 260 °C |
94.4 BTU-in/hr-ft²-°F @Temperature 500 °F |
||
| 14.7 W/m-K @Temperature 316 °C |
102 BTU-in/hr-ft²-°F @Temperature 601 °F |
||
| 16.8 W/m-K @Temperature 427 °C |
117 BTU-in/hr-ft²-°F @Temperature 801 °F |
||
| 18.8 W/m-K @Temperature 538 °C |
130 BTU-in/hr-ft²-°F @Temperature 1000 °F |
||
| 20.0 W/m-K @Temperature 593 °C |
139 BTU-in/hr-ft²-°F @Temperature 1100 °F |
||
| 21.0 W/m-K @Temperature 644 °C |
146 BTU-in/hr-ft²-°F @Temperature 1190 °F |
||
| 22.0 W/m-K @Temperature 704 °C |
153 BTU-in/hr-ft²-°F @Temperature 1300 °F |
||
| 23.1 W/m-K @Temperature 760 °C |
160 BTU-in/hr-ft²-°F @Temperature 1400 °F |
||
| 24.1 W/m-K @Temperature 816 °C |
167 BTU-in/hr-ft²-°F @Temperature 1500 °F |
||
| 25.1 W/m-K @Temperature 871 °C |
174 BTU-in/hr-ft²-°F @Temperature 1600 °F |
||
| Melting Point | 1310 - 1345 °C | 2390 - 2453 °F | |
| Solidus | 1310 °C | 2390 °F | |
| Liquidus | 1335 °C | 2435 °F |
| Component Elements Properties | Metric | English | Comments |
|---|---|---|---|
| Aluminum, Al | 1.4 - 1.6 % | 1.4 - 1.6 % | |
| Boron, B | 0.0030 - 0.010 % | 0.0030 - 0.010 % | |
| Carbon, C | 0.050 - 0.12 % | 0.050 - 0.12 % | |
| Chromium, Cr | 18 - 20 % | 18 - 20 % | |
| Cobalt, Co | 10 - 12 % | 10 - 12 % | |
| Iron, Fe | <= 5.0 % | <= 5.0 % | |
| Manganese, Mn | <= 0.10 % | <= 0.10 % | |
| Molybdenum, Mo | 9.0 - 10.5 % | 9.0 - 10.5 % | |
| Nickel, Ni | 53 % | 53 % | As Remainder |
| Silicon, Si | <= 0.50 % | <= 0.50 % |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Magnetic Permeability | <= 1.002 @Temperature 21.0 °C |
<= 1.002 @Temperature 69.8 °F |
at 200 oersteds |