| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | >= 1.40 g/cc | >= 1.40 g/cc | |
| Moisture Absorption at Equilibrium | 2.5 % @Thickness 1.57 mm |
2.5 % @Thickness 0.0620 in |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Rockwell M | 100 @Thickness 1.57 mm |
100 @Thickness 0.0620 in |
|
| Tensile Strength, Yield | 63.4 MPa @Thickness 3.17 mm |
9200 psi @Thickness 0.125 in |
CW |
| 72.4 MPa @Thickness 3.17 mm |
10500 psi @Thickness 0.125 in |
LW | |
| Flexural Strength | 93.1 MPa @Thickness 1.57 mm |
13500 psi @Thickness 0.0620 in |
CW |
| 93.1 MPa @Thickness 1.57 mm |
13500 psi @Thickness 0.0620 in |
LW | |
| Flexural Modulus | 10.3 GPa @Thickness 1.57 mm |
1500 ksi @Thickness 0.0620 in |
CW |
| 10.3 GPa @Thickness 1.57 mm |
1500 ksi @Thickness 0.0620 in |
LW | |
| Compressive Strength | 172 MPa @Thickness 12.7 mm |
25000 psi @Thickness 0.500 in |
Flatwise |
| Izod Impact, Unnotched | 0.294 J/cm @Thickness 12.7 mm |
0.550 ft-lb/in @Thickness 0.500 in |
CW, E-48/50 |
| 0.320 J/cm @Thickness 12.7 mm |
0.600 ft-lb/in @Thickness 0.500 in |
LW, E-48/50 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear | 10.0 µm/m-°C @Temperature 20.0 °C |
5.56 µin/in-°F @Temperature 68.0 °F |
x-axis |
| CTE, linear, Transverse to Flow | 14.0 µm/m-°C @Temperature 20.0 °C |
7.78 µin/in-°F @Temperature 68.0 °F |
y-axis |
| Maximum Service Temperature, Air | 120 °C | 248 °F | Maximum Operating Temperature |
| Flammability, UL94 | V-1 | V-1 |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Dielectric Breakdown | 5000 V @Thickness 1.57 mm |
5000 V @Thickness 0.0620 in |
D-48/50 |
| 50000 V @Thickness 1.57 mm |
50000 V @Thickness 0.0620 in |
Condition A | |
| Arc Resistance | 120 sec @Thickness 3.17 mm |
120 sec @Thickness 0.125 in |
ASTM D495 |
| Descriptive Properties | Value | Comments |
|---|---|---|
| Bond Strength | 1,000 lb | 0.5" |