Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Acrylonitrile Butadiene Styrene (ABS), Sheet". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 0.775 - 1.28 g/cc
0.0280 - 0.0462 lb/in³
Average value: 1.06 g/cc Grade Count:25
Linear Mold Shrinkage 0.00550 cm/cm
0.00550 in/in
Average value: 0.00550 cm/cm Grade Count:3
Melt Flow 1.20 - 2.60 g/10 min
1.20 - 2.60 g/10 min
Average value: 2.08 g/10 min Grade Count:4
Mechanical Properties Metric English Comments
Hardness, Rockwell R 80.0 - 105
80.0 - 105
Average value: 96.4 Grade Count:22
Tensile Strength, Ultimate 15.9 - 34.5 MPa
2310 - 5000 psi
Average value: 28.3 MPa Grade Count:6
Tensile Strength, Yield 31.0 - 42.7 MPa
4500 - 6200 psi
Average value: 37.3 MPa Grade Count:22
Elongation at Break 40.0 - 190 %
40.0 - 190 %
Average value: 95.0 % Grade Count:4
Modulus of Elasticity 1.83 - 2.21 GPa
265 - 320 ksi
Average value: 2.07 GPa Grade Count:12
Flexural Yield Strength 34.5 - 75.8 MPa
5000 - 11000 psi
Average value: 59.6 MPa Grade Count:21
Flexural Modulus 1.59 - 2.48 GPa
230 - 360 ksi
Average value: 2.03 GPa Grade Count:22
Izod Impact, Notched 2.40 - 5.34 J/cm
4.50 - 10.0 ft-lb/in
Average value: 3.81 J/cm Grade Count:11
0.80085 - 2.6695 J/cm

@Temperature -29.0 - -28.9 °C
1.5003 - 5.0011 ft-lb/in

@Temperature -20.2 - -20.0 °F
Average value: 1.43 J/cm Grade Count:8
Izod Impact, Unnotched 2.67 - 4.27 J/cm
5.00 - 8.00 ft-lb/in
Average value: 3.63 J/cm Grade Count:10
0.58729 - 2.1356 J/cm

@Temperature -40.0 - -40.0 °C
1.1002 - 4.0009 ft-lb/in

@Temperature -40.0 - -40.0 °F
Average value: 1.14 J/cm Grade Count:8
Falling Dart Impact 20.3 - 47.5 J
15.0 - 35.0 ft-lb
Average value: 34.3 J Grade Count:9
4.06746 - 31.1839 J

@Temperature -40.0 - -40.0 °C
3.00000 - 23.0000 ft-lb

@Temperature -40.0 - -40.0 °F
Average value: 14.6 J Grade Count:8
Thermal Properties Metric English Comments
CTE, linear 59.4 - 101 µm/m-°C
33.0 - 56.0 µin/in-°F
Average value: 88.3 µm/m-°C Grade Count:21
Deflection Temperature at 0.46 MPa (66 psi) 93.0 - 93.9 °C
199 - 201 °F
Average value: 93.2 °C Grade Count:4
Deflection Temperature at 1.8 MPa (264 psi) 77.8 - 106 °C
172 - 222 °F
Average value: 90.0 °C Grade Count:24
Vicat Softening Point 95.0 - 107 °C
203 - 225 °F
Average value: 104 °C Grade Count:4
Flammability, UL94 HB - V-0
HB - V-0
Grade Count:13
Optical Properties Metric English Comments
Gloss 16.0 - 95.0 %
16.0 - 95.0 %
Average value: 83.3 % Grade Count:12