Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Techmer ES Elastoblend® PA6/6 GF13 IM HS L 13% Glass Filled

Category Polymer , Thermoplastic , Nylon , Nylon 66 , Nylon 66, 10% Glass Fiber Filled , Nylon 66, Glass Reinforced, Impact Grade , Nylon 66, Heat Stabilized
Manufacturer Techmer ES
Trade Name Elastoblend®
Port Ningbo port,China
Trade Terms EXW, FOB, CFR, CIF
Payment Terms L/C, T/T, PayPal
Download PDF Techmer ES Elastoblend® PA6/6 GF13 IM HS L 13% Glass Filled.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Availability: North AmericaForms: PelletsFiller/Reinforcement: Glass Fiber Reinforcement, 13% Filler by WeightAdditive: Heat Stabilizer and Impact ModifierFeatures: Heat Stabilized and Impact Modified Processing Method: Injection MoldingInformation provided by TP Composites, Inc.
Physical Properties Metric English Comments
Density 1.17 g/cc
0.0423 lb/in³
ASTM D792
Water Absorption 0.80 %

@Time 86400 sec
0.80 %

@Time 24.0 hour
ASTM D570
Linear Mold Shrinkage, Flow 0.0060 cm/cm

@Thickness 3.17 mm
0.0060 in/in

@Thickness 0.125 in
ASTM D955
Mechanical Properties Metric English Comments
Hardness, Rockwell R 111
111
ASTM D785
Tensile Strength, Yield 91.0 MPa
13200 psi
ASTM D638
Elongation at Break 4.0 %
4.0 %
ASTM D638
Flexural Strength 110 MPa
16000 psi
ASTM D790
Flexural Modulus 36.2 GPa
5250 ksi
ASTM D790
Izod Impact, Notched 1.07 J/cm

@Thickness 3.17 mm,
Temperature -40.0 °C
2.00 ft-lb/in

@Thickness 0.125 in,
Temperature -40.0 °F
ASTM D256
1.60 J/cm

@Thickness 3.17 mm,
Temperature 22.8 °C
3.00 ft-lb/in

@Thickness 0.125 in,
Temperature 73.0 °F
ASTM D256
Izod Impact, Unnotched NB

@Thickness 3.17 mm
NB

@Thickness 0.125 in
ASTM D256
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 54.0 µm/m-°C
30.0 µin/in-°F
ASTM D696
Deflection Temperature at 0.46 MPa (66 psi) 252 °C
485 °F
Unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 220 °C
428 °F
Unannealed; ASTM D648
Flammability, UL94 HB
HB
Electrical Properties Metric English Comments
Volume Resistivity 1.00e+14 ohm-cm
1.00e+14 ohm-cm
ASTM D257
Dielectric Strength 19.3 kV/mm
490 kV/in
Method A (Short-Time); ASTM D149
Users viewing this material also viewed the following: