Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Braskem GV0350 HDPE Blow Molding Polyethylene Copolymer

Category Polymer , Thermoplastic , Polyethylene (PE) , HDPE , High Density Polyethylene (HDPE), Blow Molding Grade
Manufacturer Braskem
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Braskem GV0350 HDPE Blow Molding Polyethylene Copolymer.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
HDPE GV0350 is a high-density polyethylene copolymer that has great molar mass, excellent chemical resistance, and high impact resistance and stiffness. It was developed for the blow-molding of large volumes, especially for 200 L tight-head blow molded drums. Its applications include: shipping containers from 100 to 240 L, L-ring drums of 200 L, and gallons and drums for chemical and agrochemical products.
Physical Properties Metric English Comments
Density 0.952 g/cc
0.0344 lb/in³
ASTM-D792
ESCR 100% Igepal® 200 hour

@Thickness 2.00 mm,
Temperature 50.0 °C
200 hour

@Thickness 0.0787 in,
Temperature 122 °F
0.3 mm notched-plaques; ASTM-D1693
ESCR 10% Igepal® 37 hour

@Thickness 2.00 mm,
Temperature 50.0 °C
37 hour

@Thickness 0.0787 in,
Temperature 122 °F
0.3 mm notched-plaques; ASTM-D1693
Melt Flow 2.5 g/10 min

@Load 21.6 kg,
Temperature 190 °C
2.5 g/10 min

@Load 47.6 lb,
Temperature 374 °F
ASTM-D1238
Mechanical Properties Metric English Comments
Hardness, Shore D 62
62
ASTM-D2240
Tensile Strength at Break 42.0 MPa
6090 psi
ASTM-D638
Tensile Strength, Yield 26.0 MPa
3770 psi
ASTM-D638
Flexural Modulus, 1% Secant 960 MPa
139000 psi
ASTM-D790
Izod Impact, Notched 8.90 J/cm
16.7 ft-lb/in
ASTM-D256
Thermal Properties Metric English Comments
Deflection Temperature at 0.46 MPa (66 psi) 75.0 °C
167 °F
ASTM-D648
Vicat Softening Point 129 °C

@Load 1.02 kg
264 °F

@Load 2.25 lb
ASTM-D1525