Crucible Steel CPM® 154 Tool Steel

Category Metal , Ferrous Metal , Carbon Steel , Tool Steel
Manufacturer Crucible Steel
Trade Name CPM®
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Crucible Steel CPM® 154 Tool Steel.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
CPM 154 is CPM-manufactured version of Crucible’s standard 154 CM. The CPM manufacturing process produces a uniform distribution of the carbides in this grade, giving this CPM 154 easier grinding and polishing, plus better toughness, than conventional 154 CM, while retaining similar heat treat response and wear properties. CPM 154 offers better corrosion resistance, better wear resistance and better hot-hardness than 440C, plus higher toughness. For knifemakers, it offers better edge retention and chipping resistance than 440C.Information provided by Crucible Industries
Physical Properties Metric English Comments
Density 7.78 g/cc
0.281 lb/in³
Mechanical Properties Metric English Comments
Hardness, Rockwell C 62
62
austenitizied at 1900°F then quenched
63
63
austenitizied at 1900°F then quenched + freeze
51

@Tempering Temp. 566 °C
51

@Tempering Temp. 1050 °F
austenitizied at 1900°F then quenched and tempered
54

@Tempering Temp. 538 °C
54

@Tempering Temp. 1000 °F
austenitizied at 1900°F then quenched and tempered
56

@Tempering Temp. 316 °C
56

@Tempering Temp. 600 °F
austenitizied at 1900°F then quenched and tempered
56

@Tempering Temp. 427 °C
56

@Tempering Temp. 800 °F
austenitizied at 1900°F then quenched and tempered
56

@Tempering Temp. 482 °C
56

@Tempering Temp. 900 °F
austenitizied at 1900°F then quenched and tempered
59

@Tempering Temp. 204 °C
59

@Tempering Temp. 400 °F
austenitizied at 1900°F then quenched and tempered
Modulus of Elasticity 207 GPa
30000 ksi
Thermal Properties Metric English Comments
CTE, linear 7.02 µm/m-°C

@Temperature -74.0 - 21.0 °C
3.90 µin/in-°F

@Temperature -101 - 69.8 °F
7.33 µm/m-°C

@Temperature 21.0 - 38.0 °C
4.07 µin/in-°F

@Temperature 69.8 - 100 °F
10.35 µm/m-°C

@Temperature 21.0 - 149 °C
5.750 µin/in-°F

@Temperature 69.8 - 300 °F
10.91 µm/m-°C

@Temperature 21.0 - 260 °C
6.061 µin/in-°F

@Temperature 69.8 - 500 °F
Component Elements Properties Metric English Comments
Carbon, C 1.05 %
1.05 %
Chromium, Cr 14 %
14 %
Iron, Fe 80.95 %
80.95 %
as balance
Molybdenum, Mo 4.0 %
4.0 %
Descriptive Properties Value Comments
Wear Resistance 49 mg
weight loss, pin abrasion method