Crucible Steel LABELLE® Silicon #2 Tool Steel

Category Metal , Ferrous Metal , Tool Steel , Shock-Resisting Steel
Manufacturer Crucible Steel
Trade Name LABELLE®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Crucible Steel LABELLE® Silicon #2 Tool Steel.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
LaBelle Silicon #2 is a shock resisting tool steel capable of maximum toughness at relatively high hardness. It has excellent resistance to impact and battering, with good edge retention.Information provided by Crucible Industries
Physical Properties Metric English Comments
Density 7.75 g/cc
0.280 lb/in³
Mechanical Properties Metric English Comments
Hardness, Brinell 187 - 235
187 - 235
Hardness, Rockwell C 60 - 61
60 - 61
oil quenched from 1650°F
64 - 65
64 - 65
water quenched from 1600°F
44 - 45

@Tempering Temp. 538 °C
44 - 45

@Tempering Temp. 1000 °F
hardened at 1650°F then tempered
47 - 48

@Tempering Temp. 482 °C
47 - 48

@Tempering Temp. 900 °F
hardened at 1650°F then tempered
51 - 52

@Tempering Temp. 427 °C
51 - 52

@Tempering Temp. 800 °F
hardened at 1650°F then tempered
56 - 57

@Tempering Temp. 371 °C
56 - 57

@Tempering Temp. 700 °F
hardened at 1650°F then tempered
57 - 58

@Tempering Temp. 316 °C
57 - 58

@Tempering Temp. 600 °F
hardened at 1650°F then tempered
58 - 59

@Tempering Temp. 260 °C
58 - 59

@Tempering Temp. 500 °F
hardened at 1650°F then tempered
58 - 60

@Tempering Temp. 204 °C
58 - 60

@Tempering Temp. 400 °F
hardened at 1650°F then tempered
60 - 61

@Tempering Temp. 149 °C
60 - 61

@Tempering Temp. 300 °F
hardened at 1650°F then tempered
Modulus of Elasticity 207 GPa
30000 ksi
Charpy Impact 66.4 J

@Tempering Temp. 149 °C
49.0 ft-lb

@Tempering Temp. 300 °F
hardened at 1650°F then tempered; C-notch
187 J

@Tempering Temp. 204 °C
138 ft-lb

@Tempering Temp. 400 °F
hardened at 1650°F then tempered; C-notch
193 J

@Tempering Temp. 316 °C
142 ft-lb

@Tempering Temp. 600 °F
hardened at 1650°F then tempered; C-notch
198 J

@Tempering Temp. 260 °C
146 ft-lb

@Tempering Temp. 500 °F
hardened at 1650°F then tempered; C-notch
212 J

@Tempering Temp. 371 °C
156 ft-lb

@Tempering Temp. 700 °F
hardened at 1650°F then tempered; C-notch
Thermal Properties Metric English Comments
CTE, linear 12.6 µm/m-°C

@Temperature 21.1 - 427 °C
7.00 µin/in-°F

@Temperature 70.0 - 800 °F
13.3 µm/m-°C

@Temperature 21.1 - 538 °C
7.40 µin/in-°F

@Temperature 70.0 - 1000 °F
13.7 µm/m-°C

@Temperature 21.1 - 649 °C
7.60 µin/in-°F

@Temperature 70.0 - 1200 °F
Thermal Conductivity 33.0 W/m-K

@Temperature 95.0 °C
229 BTU-in/hr-ft²-°F

@Temperature 203 °F
Component Elements Properties Metric English Comments
Carbon, C 0.60 %
0.60 %
Chromium, Cr 0.25 %
0.25 %
Iron, Fe 95.9 %
95.9 %
as balance
Manganese, Mn 0.85 %
0.85 %
Molybdenum, Mo 0.30 %
0.30 %
Silicon, Si 1.9 %
1.9 %
Vanadium, V 0.20 %
0.20 %
Chemical Properties Metric English Comments
Critical Temperature 766 °C
1410 °F