Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Latrobe Lescalloy® AF 1410 VIM-VAR ; 9 in High Strength Alloy Steel

Category Metal , Ferrous Metal , Alloy Steel , Carbon Steel , High Carbon Steel
Manufacturer Latrobe Steel
Trade Name Lescalloy®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Latrobe Lescalloy® AF 1410 VIM-VAR ; 9 in High Strength Alloy Steel.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
LESCALLOY AF1410 VIM-VAR steel exhibits both high strength and very high fracture toughness. It is typically used in the 235/260 ksi (1620/1793 MPa) tensile strength range for a variety of critical, fracture-sensitive aerospace structural applications. It is double vacuum melted (VIM-VAR…vacuum induction melted followed by vacuum arc remelting) to provide superior cleanliness, ingot homogeneity, and to enhance mechanical properties.Heat Treatment - 857°C - 1 hour oil quench; -73°C - 1 hr air warm; 510°C - 5 hrs air coolInformation Provided by Timken Latrobe Steel.Timken sold Latrobe in December 2006. They are now Latrobe Specialty Steels Co.
Physical Properties Metric English Comments
Density 7.83 g/cc
0.283 lb/in³
Mechanical Properties Metric English Comments
Tensile Strength, Ultimate 1660 MPa
241000 psi
Transverse
1660 MPa
241000 psi
Longitudinal
Tensile Strength, Yield 1517 MPa
220000 psi
Longitudinal
1524 MPa
221000 psi
Transverse
Elongation at Break 16 %
16 %
Transverse
17 %
17 %
Longitudinal
Reduction of Area 68 %
68 %
Transverse
72 %
72 %
Longitudinal
Modulus of Elasticity 203 GPa
29400 ksi
Charpy Impact 71.0 J
52.4 ft-lb
V-Notch, Transverse
83.0 J
61.2 ft-lb
V-Notch, Longitudinal
Component Elements Properties Metric English Comments
Carbon, C 0.15 %
0.15 %
Chromium, Cr 2.0 %
2.0 %
Cobalt, Co 14 %
14 %
Iron, Fe 72.65 %
72.65 %
Manganese, Mn 0.10 %
0.10 %
Molybdenum, Mo 1.0 %
1.0 %
Nickel, Ni 10 %
10 %
Silicon, Si 0.10 %
0.10 %
Chemical Properties Metric English Comments
Critical Temperature 168 °C
334 °F
Martensitic Finish
336 °C
637 °F
Martensitic Start