Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Styron CALIBREâ„¢ 200 15 Polycarbonate, General Purpose

Category Polymer , Thermoplastic , Polycarbonate (PC) , Polycarbonate, Unreinforced, Flame Retardant
Manufacturer Styron
Trade Name CALIBRE™
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Styron CALIBREâ„¢ 200 15 Polycarbonate, General Purpose.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
CALIBRE® 200 series are general purpose, UL listed Polycarbonate resins formulated to comply with the applicable FDA and European regulations governing food contact(1). CALIBRE 200 series resins exhibit an excellent physical property balance of heat resistance, transparency and impact strength. The CALIBRE 200 series can be supplied with a mold release package, a UV stabilizer package or both.The CALIBRE 200 series resins are typically used for food processors, liquid containers and food utensils.Available Melt Flow Rates: 4, 6, 10, 15, 22.Associated products: CALIBRE 200: without a mold release and UV stabilization package CALIBRE 201: including a mold release package CALIBRE 202: including a UV stabilizer package CALIBRE 203: including a mold release and UV stabilizer package.(1) When used unmodified for the manufacture of food contact articles CALIBRE 200 series Polycarbonate resins comply with the U.S. Food, Drug and Cosmetic Act and Food Additive Regulations 21 CFR 177.1580 and most European regulations. The regulations should be consulted for complete details.Data provided by Dow Chemical.This product line was spun off from Dow Chemical to Styron in 2010.
Physical Properties Metric English Comments
Density 1.20 g/cc
0.0434 lb/in³
ASTM Data
Water Absorption 0.15 %
0.15 %
Moisture Absorption at Equilibrium 0.32 %
0.32 %
Humidity Absorption
Linear Mold Shrinkage 0.0060 cm/cm
0.0060 in/in
Melt Flow 15 g/10 min

@Load 1.20 kg,
Temperature 300 °C
15 g/10 min

@Load 2.65 lb,
Temperature 572 °F
ASTM Data
Mechanical Properties Metric English Comments
Hardness, Rockwell R 118
118
Tensile Strength, Ultimate 71.0 MPa
10300 psi
ASTM Data
Tensile Strength, Yield 62.1 MPa
9010 psi
ASTM Data
Elongation at Break 150 %
150 %
ASTM Data
Elongation at Yield 6.0 %
6.0 %
ISO Data
Tensile Modulus 2.34 GPa
339 ksi
ASTM Data
Izod Impact, Notched 8.54 J/cm
16.0 ft-lb/in
ASTM Data
Izod Impact, Unnotched NB
NB
ASTM Data
Charpy Impact Unnotched NB
NB
ISO Data
NB
NB
ISO Data, Low Temp
Charpy Impact, Notched 1.20 J/cm²
5.71 ft-lb/in²
ISO Data, Low Temp
8.00 J/cm²
38.1 ft-lb/in²
ISO Data
Tensile Impact Strength 462 kJ/m²
220 ft-lb/in²
ASTM Data
Impact Test 87.0 J

@Temperature 23.0 °C
64.2 ft-lb

@Temperature 73.4 °F
Instrumented Dart Total Energy
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 68.4 µm/m-°C

@Temperature 20.0 °C
38.0 µin/in-°F

@Temperature 68.0 °F
ASTM data
Deflection Temperature at 1.8 MPa (264 psi) 127 °C
261 °F
Unannealed; ASTM Data
Vicat Softening Point 154 °C
309 °F
Flammability, UL94 V-2

@Thickness 3.20 mm
V-2

@Thickness 0.126 in
Oxygen Index 26 %
26 %
Optical Properties Metric English Comments
Haze 1.1 %
1.1 %
Transmission, Visible 89 %
89 %
Electrical Properties Metric English Comments
Electrical Resistivity 2.00e+17 ohm-cm
2.00e+17 ohm-cm
ASTM Data
Dielectric Constant 2.93

@Frequency 60 Hz
2.93

@Frequency 60 Hz
ASTM Data
2.93

@Frequency 1e+6 Hz
2.93

@Frequency 1e+6 Hz
ASTM Data
Dielectric Strength 16.5 kV/mm
419 kV/in
Dissipation Factor 0.00050

@Frequency 60 Hz
0.00050

@Frequency 60 Hz
0.0017

@Frequency 1e+6 Hz
0.0017

@Frequency 1e+6 Hz
ASTM Data