| Category | Polymer , Thermoplastic , Nylon , Nylon 66 , Nylon 66, 40% Glass Fiber Filled |
| Manufacturer | DuPont Performance Polymers |
| Trade Name | Zytel® |
| Port | Ningbo port,China |
| Trade Terms | FOB, CFR, CIF |
| Payment Terms | L/C, T/T, Western Union |
| Download PDF | DuPont Performance Polymers Zytel® 70G35HSRX BK099 Nylon 66
(Unverified Data**).pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.24 g/cc | 0.0448 lb/in³ | |
| 1.41 g/cc | 0.0509 lb/in³ | DAM; ISO 1183 | |
| Water Absorption | 5.5 % @Thickness 2.00 mm |
5.5 % @Thickness 0.0787 in |
DAM; Sim. to ISO 62 |
| Moisture Absorption | 1.70 % @Thickness 2.00 mm |
1.70 % @Thickness 0.0787 in |
DAM; Sim. to ISO 62 |
| Viscosity | 66620 cP @Shear Rate 5000 1/s, Temperature 305 °C |
66620 cP @Shear Rate 5000 1/s, Temperature 581 °F |
ISO 11403-1 -2 |
| 81170 cP @Shear Rate 5000 1/s, Temperature 295 °C |
81170 cP @Shear Rate 5000 1/s, Temperature 563 °F |
ISO 11403-1 -2 | |
| 100580 cP @Shear Rate 5000 1/s, Temperature 285 °C |
100580 cP @Shear Rate 5000 1/s, Temperature 545 °F |
ISO 11403-1 -2 | |
| 200700 cP @Shear Rate 500 1/s, Temperature 305 °C |
200700 cP @Shear Rate 500 1/s, Temperature 581 °F |
ISO 11403-1 -2 | |
| 253900 cP @Shear Rate 500 1/s, Temperature 295 °C |
253900 cP @Shear Rate 500 1/s, Temperature 563 °F |
ISO 11403-1 -2 | |
| 323800 cP @Shear Rate 500 1/s, Temperature 285 °C |
323800 cP @Shear Rate 500 1/s, Temperature 545 °F |
ISO 11403-1 -2 | |
| Viscosity Test | 150 cm³/g | 150 cm³/g | DAM; ISO 307 1157 1628 |
| Linear Mold Shrinkage, Flow | 0.0030 cm/cm | 0.0030 in/in | DAM; ISO 294-4 2577 |
| Linear Mold Shrinkage, Transverse | 0.011 cm/cm | 0.011 in/in | DAM; ISO 294-4 2577 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Ball Indentation Hardness | 285 MPa | 41300 psi | DAM; H 961/30; ISO 2039-1 |
| Tensile Strength at Break | 150 MPa | 21800 psi | 50%RH; ISO 527-1/-2 |
| 210 MPa | 30500 psi | DAM; ISO 527-1/-2 | |
| Tensile Stress | 7.49 MPa @Strain 0.190 %, Temperature 150 °C |
1090 psi @Strain 0.190 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 |
| 9.23 MPa @Strain 0.220 %, Temperature 180 °C |
1340 psi @Strain 0.220 %, Temperature 356 °F |
DAM; ISO 11403-1 -2 | |
| 12.19 MPa @Strain 0.220 %, Temperature 90.0 °C |
1768 psi @Strain 0.220 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 14.47 MPa @Strain 0.240 %, Temperature 90.0 °C |
2099 psi @Strain 0.240 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 16.86 MPa @Strain 0.250 %, Temperature 40.0 °C |
2445 psi @Strain 0.250 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 17.67 MPa @Strain 0.230 %, Temperature 23.0 °C |
2563 psi @Strain 0.230 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 18.42 MPa @Strain 0.400 %, Temperature 150 °C |
2672 psi @Strain 0.400 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 28.36 MPa @Strain 0.290 %, Temperature 0.000 °C |
4113 psi @Strain 0.290 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 28.62 MPa @Strain 0.260 %, Temperature 40.0 °C |
4151 psi @Strain 0.260 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 32.65 MPa @Strain 1.13 %, Temperature 150 °C |
4735 psi @Strain 1.13 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 39.21 MPa @Strain 0.310 %, Temperature 0.000 °C |
5687 psi @Strain 0.310 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 40.07 MPa @Strain 0.900 %, Temperature 90.0 °C |
5812 psi @Strain 0.900 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 42.44 MPa @Strain 1.61 %, Temperature 180 °C |
6155 psi @Strain 1.61 %, Temperature 356 °F |
DAM; ISO 11403-1 -2 | |
| 46.29 MPa @Strain 0.360 %, Temperature -20.0 °C |
6714 psi @Strain 0.360 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |
| 50.25 MPa @Strain 1.49 %, Temperature 150 °C |
7288 psi @Strain 1.49 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 50.93 MPa @Strain 1.01 %, Temperature 90.0 °C |
7387 psi @Strain 1.01 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 51.91 MPa @Strain 0.780 %, Temperature 23.0 °C |
7529 psi @Strain 0.780 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 52.11 MPa @Strain 0.920 %, Temperature 40.0 °C |
7558 psi @Strain 0.920 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 52.39 MPa @Strain 2.42 %, Temperature 150 °C |
7599 psi @Strain 2.42 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 60.88 MPa @Strain 3.24 %, Temperature 180 °C |
8830 psi @Strain 3.24 %, Temperature 356 °F |
DAM; ISO 11403-1 -2 | |
| 63.15 MPa @Strain 0.560 %, Temperature 23.0 °C |
9159 psi @Strain 0.560 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 65.51 MPa @Strain 4.00 %, Temperature 150 °C |
9501 psi @Strain 4.00 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 66.01 MPa @Strain 1.85 %, Temperature 90.0 °C |
9574 psi @Strain 1.85 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 66.32 MPa @Strain 0.490 %, Temperature -20.0 °C |
9619 psi @Strain 0.490 %, Temperature -4.00 °F |
DAM; ISO 11403-1 -2 | |
| 69.5 MPa @Strain 0.760 %, Temperature 0.000 °C |
10100 psi @Strain 0.760 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 72.35 MPa @Strain 5.03 %, Temperature 180 °C |
10490 psi @Strain 5.03 %, Temperature 356 °F |
DAM; ISO 11403-1 -2 | |
| 72.59 MPa @Strain 2.90 %, Temperature 150 °C |
10530 psi @Strain 2.90 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 74.0 MPa @Strain 0.700 %, Temperature 40.0 °C |
10700 psi @Strain 0.700 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 80.93 MPa @Strain 1.99 %, Temperature 90.0 °C |
11740 psi @Strain 1.99 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 84.39 MPa @Strain 3.11 %, Temperature 90.0 °C |
12240 psi @Strain 3.11 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 84.44 MPa @Strain 1.79 %, Temperature 40.0 °C |
12250 psi @Strain 1.79 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 86.41 MPa @Strain 4.58 %, Temperature 150 °C |
12530 psi @Strain 4.58 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 87.82 MPa @Strain 1.57 %, Temperature 23.0 °C |
12740 psi @Strain 1.57 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 93.47 MPa @Strain 0.820 %, Temperature -20.0 °C |
13560 psi @Strain 0.820 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |
| 97.09 MPa @Strain 0.810 %, Temperature 0.000 °C |
14080 psi @Strain 0.810 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 105.38 MPa @Strain 3.18 %, Temperature 90.0 °C |
15284 psi @Strain 3.18 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 108.13 MPa @Strain 2.82 %, Temperature 40.0 °C |
15683 psi @Strain 2.82 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 108.59 MPa @Strain 1.31 %, Temperature 0.000 °C |
15750 psi @Strain 1.31 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 110.68 MPa @Strain 1.02 %, Temperature 23.0 °C |
16053 psi @Strain 1.02 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 115.45 MPa @Strain 2.44 %, Temperature 23.0 °C |
16745 psi @Strain 2.44 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 116.32 MPa @Strain 1.23 %, Temperature 40.0 °C |
16871 psi @Strain 1.23 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 125.68 MPa @Strain 0.990 %, Temperature -20.0 °C |
18228 psi @Strain 0.990 %, Temperature -4.00 °F |
DAM; ISO 11403-1 -2 | |
| 136.46 MPa @Strain 1.30 %, Temperature -20.0 °C |
19792 psi @Strain 1.30 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |
| 145.9 MPa @Strain 2.02 %, Temperature 0.000 °C |
21160 psi @Strain 2.02 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 146.62 MPa @Strain 1.32 %, Temperature 0.000 °C |
21265 psi @Strain 1.32 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 153.73 MPa @Strain 1.55 %, Temperature 23.0 °C |
22297 psi @Strain 1.55 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 154.52 MPa @Strain 1.95 %, Temperature 40.0 °C |
22411 psi @Strain 1.95 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 176.66 MPa @Strain 1.55 %, Temperature -20.0 °C |
25622 psi @Strain 1.55 %, Temperature -4.00 °F |
DAM; ISO 11403-1 -2 |