| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 8.98 g/cc | 0.324 lb/in³ | at RT. |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Brinell | 269 | 269 | Converted from Rockwell C hardness. |
| Hardness, Knoop | 300 | 300 | Converted from Rockwell C hardness. |
| Hardness, Rockwell C | 27.8 | 27.8 | |
| Hardness, Vickers | 286 | 286 | Converted from Rockwell C hardness. |
| Tensile Strength, Ultimate | 1055 MPa | 153000 psi | |
| Tensile Strength, Yield | 605 MPa <br>@Strain 0.200 % |
87700 psi <br>@Strain 0.200 % |
|
| Elongation at Break | 41 % | 41 % | in 51 mm |
| Modulus of Elasticity | 232 GPa | 33600 ksi | RT |
| 153 GPa <br>@Temperature 1000 °C |
22200 ksi <br>@Temperature 1830 °F |
||
| 161 GPa <br>@Temperature 900 °C |
23400 ksi <br>@Temperature 1650 °F |
||
| 169 GPa <br>@Temperature 800 °C |
24500 ksi <br>@Temperature 1470 °F |
||
| 176 GPa <br>@Temperature 700 °C |
25500 ksi <br>@Temperature 1290 °F |
||
| 184 GPa <br>@Temperature 600 °C |
26700 ksi <br>@Temperature 1110 °F |
||
| 193 GPa <br>@Temperature 500 °C |
28000 ksi <br>@Temperature 932 °F |
||
| 201 GPa <br>@Temperature 400 °C |
29200 ksi <br>@Temperature 752 °F |
||
| 209 GPa <br>@Temperature 300 °C |
30300 ksi <br>@Temperature 572 °F |
||
| 217 GPa <br>@Temperature 200 °C |
31500 ksi <br>@Temperature 392 °F |
||
| 225 GPa <br>@Temperature 100 °C |
32600 ksi <br>@Temperature 212 °F |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear | 11.9 µm/m-°C <br>@Temperature 25.0 - 100 °C |
6.61 µin/in-°F <br>@Temperature 77.0 - 212 °F |
|
| 12.6 µm/m-°C <br>@Temperature 25.0 - 200 °C |
7.00 µin/in-°F <br>@Temperature 77.0 - 392 °F |
||
| 13.2 µm/m-°C <br>@Temperature 25.0 - 300 °C |
7.33 µin/in-°F <br>@Temperature 77.0 - 572 °F |
||
| 13.8 µm/m-°C <br>@Temperature 25.0 - 400 °C |
7.67 µin/in-°F <br>@Temperature 77.0 - 752 °F |
||
| 14.5 µm/m-°C <br>@Temperature 25.0 - 500 °C |
8.06 µin/in-°F <br>@Temperature 77.0 - 932 °F |
||
| 15.2 µm/m-°C <br>@Temperature 25.0 - 600 °C |
8.44 µin/in-°F <br>@Temperature 77.0 - 1110 °F |
||
| 15.8 µm/m-°C <br>@Temperature 25.0 - 700 °C |
8.78 µin/in-°F <br>@Temperature 77.0 - 1290 °F |
||
| 16.5 µm/m-°C <br>@Temperature 25.0 - 800 °C |
9.17 µin/in-°F <br>@Temperature 77.0 - 1470 °F |
||
| 17.1 µm/m-°C <br>@Temperature 25.0 - 800 °C |
9.50 µin/in-°F <br>@Temperature 77.0 - 1470 °F |
||
| 17.9 µm/m-°C <br>@Temperature 25.0 - 1000 °C |
9.94 µin/in-°F <br>@Temperature 77.0 - 1830 °F |
||
| Specific Heat Capacity | 0.403 J/g-°C | 0.0963 BTU/lb-°F | RT |
| 0.423 J/g-°C <br>@Temperature 100 °C |
0.101 BTU/lb-°F <br>@Temperature 212 °F |
||
| 0.444 J/g-°C <br>@Temperature 200 °C |
0.106 BTU/lb-°F <br>@Temperature 392 °F |
||
| 0.465 J/g-°C <br>@Temperature 300 °C |
0.111 BTU/lb-°F <br>@Temperature 572 °F |
||
| 0.486 J/g-°C <br>@Temperature 400 °C |
0.116 BTU/lb-°F <br>@Temperature 752 °F |
||
| 0.502 J/g-°C <br>@Temperature 500 °C |
0.120 BTU/lb-°F <br>@Temperature 932 °F |
||
| 0.523 J/g-°C <br>@Temperature 600 °C |
0.125 BTU/lb-°F <br>@Temperature 1110 °F |
||
| 0.540 J/g-°C <br>@Temperature 700 °C |
0.129 BTU/lb-°F <br>@Temperature 1290 °F |
||
| 0.557 J/g-°C <br>@Temperature 800 °C |
0.133 BTU/lb-°F <br>@Temperature 1470 °F |
||
| 0.573 J/g-°C <br>@Temperature 900 °C |
0.137 BTU/lb-°F <br>@Temperature 1650 °F |
||
| 0.590 J/g-°C <br>@Temperature 1000 °C |
0.141 BTU/lb-°F <br>@Temperature 1830 °F |
||
| Thermal Conductivity | 10.4 W/m-K | 72.2 BTU-in/hr-ft²-°F | RT |
| 12.2 W/m-K <br>@Temperature 100 °C |
84.7 BTU-in/hr-ft²-°F <br>@Temperature 212 °F |
||
| 14.3 W/m-K <br>@Temperature 200 °C |
99.2 BTU-in/hr-ft²-°F <br>@Temperature 392 °F |
||
| 15.9 W/m-K <br>@Temperature 300 °C |
110 BTU-in/hr-ft²-°F <br>@Temperature 572 °F |
||
| 17.5 W/m-K <br>@Temperature 400 °C |
121 BTU-in/hr-ft²-°F <br>@Temperature 752 °F |
||
| 19.3 W/m-K <br>@Temperature 500 °C |
134 BTU-in/hr-ft²-°F <br>@Temperature 932 °F |
||
| 21.1 W/m-K <br>@Temperature 600 °C |
146 BTU-in/hr-ft²-°F <br>@Temperature 1110 °F |
||
| 23.0 W/m-K <br>@Temperature 700 °C |
160 BTU-in/hr-ft²-°F <br>@Temperature 1290 °F |
||
| 24.8 W/m-K <br>@Temperature 800 °C |
172 BTU-in/hr-ft²-°F <br>@Temperature 1470 °F |
||
| 25.5 W/m-K <br>@Temperature 900 °C |
177 BTU-in/hr-ft²-°F <br>@Temperature 1650 °F |
||
| 27.6 W/m-K <br>@Temperature 1000 °C |
192 BTU-in/hr-ft²-°F <br>@Temperature 1830 °F |
||
| Melting Point | 1315 - 1410 °C | 2399 - 2570 °F | |
| Solidus | 1315 °C | 2399 °F | |
| Liquidus | 1410 °C | 2570 °F | |
| Maximum Service Temperature, Air | 1095 °C | 2003 °F |
| Component Elements Properties | Metric | English | Comments |
|---|---|---|---|
| Boron, B | <= 0.015 % | <= 0.015 % | |
| Carbon, C | 0.050 - 0.15 % | 0.050 - 0.15 % |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Electrical Resistivity | 0.000101 ohm-cm | 0.000101 ohm-cm | RT |
| 0.000103 ohm-cm <br>@Temperature 100 °C |
0.000103 ohm-cm <br>@Temperature 212 °F |
||
| 0.000105 ohm-cm <br>@Temperature 200 °C |
0.000105 ohm-cm <br>@Temperature 392 °F |
||
| 0.0001077 ohm-cm <br>@Temperature 300 °C |
0.0001077 ohm-cm <br>@Temperature 572 °F |
||
| 0.0001105 ohm-cm <br>@Temperature 400 °C |
0.0001105 ohm-cm <br>@Temperature 752 °F |
||
| 0.0001127 ohm-cm <br>@Temperature 500 °C |
0.0001127 ohm-cm <br>@Temperature 932 °F |
||
| 0.0001148 ohm-cm <br>@Temperature 600 °C |
0.0001148 ohm-cm <br>@Temperature 1110 °F |
||
| 0.0001164 ohm-cm <br>@Temperature 700 °C |
0.0001164 ohm-cm <br>@Temperature 1290 °F |
||
| 0.0001175 ohm-cm <br>@Temperature 800 °C |
0.0001175 ohm-cm <br>@Temperature 1470 °F |
||
| 0.0001183 ohm-cm <br>@Temperature 900 °C |
0.0001183 ohm-cm <br>@Temperature 1650 °F |
||
| 0.0001191 ohm-cm <br>@Temperature 1000 °C |
0.0001191 ohm-cm <br>@Temperature 1830 °F |