| Category | Polymer , Thermoplastic , Polycarbonate (PC) |
| Manufacturer | SABIC Innovative Plastics (GE Plastics) |
| Trade Name | LNP STAT-KON |
| Port | Shanghai port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | SABIC Innovative Plastics LNP STAT-KON DEP23FXC PC (Asia Pacific).pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.28 g/cc | 0.0462 lb/in³ | ISO 1183 |
| 1.29 g/cc | 0.0466 lb/in³ | ASTM D792 | |
| Moisture Absorption | 0.120 % | 0.120 % | 50% RH, 24 hrs; ASTM D570 |
| Linear Mold Shrinkage, Flow | 0.0016 cm/cm @Time 86400 sec |
0.0016 in/in @Time 24.0 hour |
ISO 294 |
| 0.0020 cm/cm @Time 86400 sec |
0.0020 in/in @Time 24.0 hour |
ASTM D955 | |
| Linear Mold Shrinkage, Transverse | 0.0027 cm/cm @Time 86400 sec |
0.0027 in/in @Time 24.0 hour |
ISO 294 |
| 0.0030 cm/cm @Time 86400 sec |
0.0030 in/in @Time 24.0 hour |
ASTM D955 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 120 MPa | 17400 psi | ASTM D638 |
| 122 MPa | 17700 psi | ISO 527 | |
| Elongation at Break | 1.8 % | 1.8 % | ISO 527 |
| 2.0 % | 2.0 % | ASTM D638 | |
| Tensile Modulus | 10.2 GPa | 1480 ksi | 1 mm/min; ISO 527 |
| 10.54 GPa | 1529 ksi | 50 mm/min; ASTM D638 | |
| Flexural Strength | 186 MPa | 27000 psi | ASTM D790 |
| 186 MPa | 27000 psi | ISO 178 | |
| Flexural Modulus | 9.10 GPa | 1320 ksi | ASTM D790 |
| 10.3 GPa | 1490 ksi | ISO 178 | |
| Izod Impact, Notched | 0.640 J/cm | 1.20 ft-lb/in | ASTM D256 |
| Izod Impact, Unnotched | 4.11 J/cm | 7.70 ft-lb/in | ASTM D4812 |
| Izod Impact, Notched (ISO) | 7.00 kJ/m² | 3.33 ft-lb/in² | 80*10*4; ISO 180/1A |
| Izod Impact, Unnotched (ISO) | 27.0 kJ/m² | 12.8 ft-lb/in² | 80*10*4; ISO 180/1U |
| Dart Drop, Total Energy | 16.0 J | 11.8 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
| Impact Test | 3.00 J | 2.21 ft-lb | Multiaxial Impact; ISO 6603 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 36.5 µm/m-°C @Temperature -40.0 - 40.0 °C |
20.3 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 |
| 36.5 µm/m-°C @Temperature -40.0 - 40.0 °C |
20.3 µin/in-°F @Temperature -40.0 - 104 °F |
ISO 11359-2 | |
| CTE, linear, Transverse to Flow | 33.3 µm/m-°C @Temperature -40.0 - 40.0 °C |
18.5 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 |
| 33.3 µm/m-°C @Temperature -40.0 - 40.0 °C |
18.5 µin/in-°F @Temperature -40.0 - 104 °F |
ISO 11359-2 | |
| Deflection Temperature at 0.46 MPa (66 psi) | 141 °C | 286 °F | Flatw 80*10*4 sp=64mm; ISO 75/Bf |
| 141 °C @Thickness 3.20 mm |
286 °F @Thickness 0.126 in |
unannealed; ASTM D648 | |
| Deflection Temperature at 1.8 MPa (264 psi) | 137 °C | 279 °F | Flatw 80*10*4 sp=64mm; ISO 75/Af |
| 137 °C @Thickness 3.20 mm |
279 °F @Thickness 0.126 in |
unannealed; ASTM D648 | |
| Flammability, UL94 | HB @Thickness 1.50 mm |
HB @Thickness 0.0591 in |
UL 94 by SABIC-IP |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Surface Resistance | 10 - 1.00e+6 ohm | 10 - 1.00e+6 ohm | ASTM D257 |