Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

SABIC Innovative Plastics Lexan® FL900P PC (Europe-Africa-Middle East)

Category Polymer , Thermoplastic , Polycarbonate (PC)
Manufacturer SABIC Innovative Plastics (GE Plastics)
Trade Name Lexan®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF SABIC Innovative Plastics Lexan® FL900P PC (Europe-Africa-Middle East).pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Foamable LEXAN, various weight reductions at 6.4 mm. Offers load bearing capability at elavated temp., Combines rigidity, impact & toughness.This data was supplied by SABIC-IP for the Europe-Africa-Middle East region.
Physical Properties Metric English Comments
Specific Gravity 0.950 g/cc
0.950 g/cc
ASTM D 792
Filler Content 5 %
5 %
ASTM D 229
Water Absorption 0.15 %

@Time 86400 sec
0.15 %

@Time 24.0 hour
ASTM D 570
Water Absorption at Saturation 0.35 %

@Temperature 23.0 °C
0.35 %

@Temperature 73.4 °F
ISO 62
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm
0.0050 - 0.0070 in/in
on tensile bar; SABIC Method
Melt Flow 10 g/10 min

@Load 1.20 kg,
Temperature 300 °C
10 g/10 min

@Load 2.65 lb,
Temperature 572 °F
[cm^3/10 min] Melt Volume Rate; ISO 1133
Mechanical Properties Metric English Comments
Tensile Strength at Break 42.0 MPa
6090 psi
5 mm/min; ISO 527
Elongation at Break 4.0 %
4.0 %
5 mm/min; ISO 527
Tensile Modulus 2.00 GPa
290 ksi
1 mm/min; ISO 527
Flexural Strength 50.0 MPa
7250 psi
2 mm/min; ISO 178
Flexural Modulus 2.20 GPa
319 ksi
2 mm/min; ISO 178
Gardner Impact 50.0 J
36.9 ft-lb
SABIC Method
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 35.0 µm/m-°C

@Temperature 23.0 - 80.0 °C
19.4 µin/in-°F

@Temperature 73.4 - 176 °F
ISO 11359-2
Specific Heat Capacity 0.280 J/g-°C
0.0669 BTU/lb-°F
ASTM C 351
Thermal Conductivity 0.150 W/m-K
1.04 BTU-in/hr-ft²-°F
ISO 8302
Flammability, UL94 V-0

@Thickness 6.00 mm
V-0

@Thickness 0.236 in
UL 94
5VA

@Thickness 6.00 mm
5VA

@Thickness 0.236 in
UL 94
Electrical Properties Metric English Comments
Dielectric Constant 2.3

@Frequency 1.00e+6 Hz
2.3

@Frequency 1.00e+6 Hz
IEC 60250
2.4

@Frequency 100 Hz
2.4

@Frequency 100 Hz
IEC 60250
Dissipation Factor 0.0029

@Frequency 100 Hz
0.0029

@Frequency 100 Hz
IEC 60250
0.010

@Frequency 1.00e+6 Hz
0.010

@Frequency 1.00e+6 Hz
IEC 60250
Descriptive Properties Value Comments
Ball Pressure Test, 125°C +/- 2°C PASSES
IEC 60695-10-2
Ball Pressure Test, 75°C +/- 2°C PASSES
IEC 60695-10-2
Copyright © lookpolymers.com All Rights Reserved