Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

TIMET TIMETAL® 1100 Titanium Alloy (Ti-6Al-2.7Sn-4Zr-0.4Mo-0.45Si)

Category Metal , Nonferrous Metal , Titanium Alloy , Alpha/Near Alpha Titanium Alloy
Manufacturer TIMET
Trade Name TIMETAL®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF TIMET TIMETAL® 1100 Titanium Alloy (Ti-6Al-2.7Sn-4Zr-0.4Mo-0.45Si).pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Features: A near alpha, high temperature creep resistant alloy developed for elevated temperature use in the range of 600°C that offers the highest combination of strength, creep resistance, fracture toughness and fatigue crack growth resistance.Data provided by TIMET.
Physical Properties Metric English Comments
Density 4.50 g/cc
0.163 lb/in³
Typical
Mechanical Properties Metric English Comments
Tensile Strength, Ultimate 1000 MPa
145000 psi
Typical
Tensile Strength, Yield 910 MPa

@Strain 0.200 %
132000 psi

@Strain 0.200 %
Typical
Elongation at Break 8.0 %
8.0 %
Typical
Modulus of Elasticity 120 GPa
17400 ksi
Typical
Fatigue Strength 500 MPa
72500 psi
Limit; test specifics not reported
Bend Radius, Minimum 6.0 t
6.0 t
Typical; on 0.078 in (2 mm) sheet
Thermal Properties Metric English Comments
Maximum Service Temperature, Air 600 °C
1110 °F
Beta Transus 1015 °C
1859 °F
Component Elements Properties Metric English Comments
Aluminum, Al 6.0 %
6.0 %
Molybdenum, Mo 0.40 %
0.40 %
Silicon, Si 0.45 %
0.45 %
Tin, Sn 2.7 %
2.7 %
Titanium, Ti 86.5 %
86.5 %
Calculated as remainder
Zirconium, Zr 4.0 %
4.0 %