Material Notes:
3M™ Screen Printable Sheet Polyester Label Material 7907 is a durable, high performance material that offers excellent thermal stability, moisture resistance and chemical resistance. This label material utilizes 3M™ Adhesive 350, which is designed to permanently bond to high and low surface energy plastics, textured and contoured surfaces, powder coatings, and slightly oily metals.Information provided by 3M
Physical Properties Metric English Comments
Thickness 45.7 microns
1.80 mil
Adhesive
58.4 microns
2.30 mil
Facestock
170 microns
6.70 mil
Liner
Mechanical Properties Metric English Comments
Peel Strength 0.1424 kN/m
0.8125 pli
LD Polyethylene, 90° Peel, Conditioned for 3 days at 49°C; ASTM D3330
0.153 kN/m
0.875 pli
LD Polyethylene, 180° Peel, Conditioned for 3 days at 49°C; ASTM D3330
0.2849 kN/m
1.625 pli
Finely Textured Powder Coating, 90° Peel, Conditioned for 3 days at RT; ASTM D3330
0.29582 kN/m
1.6875 pli
Finely Textured Powder Coating, 90° Peel, Initial, 10 min dwell at RT; ASTM D3330
0.307 kN/m
1.75 pli
HD Polyethylene, 90° Peel, Initial, 10 min dwell at RT; ASTM D3330
0.307 kN/m
1.75 pli
Finely Textured Powder Coating, 90° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
0.31773 kN/m
1.8125 pli
LD Polyethylene, 90° Peel, Initial, 10 min dwell at RT; ASTM D3330
0.31773 kN/m
1.8125 pli
Polypropylene, 90° Peel, Conditioned for 3 days at RT; ASTM D3330
0.3287 kN/m
1.875 pli
Polypropylene, 90° Peel, Initial, 10 min dwell at RT; ASTM D3330
0.3287 kN/m
1.875 pli
HD Polyethylene, 90° Peel, Conditioned for 3 days at 49°C; ASTM D3330
0.351 kN/m
2.00 pli
HD Polyethylene, 90° Peel, Conditioned for 3 days at RT; ASTM D3330
0.36156 kN/m
2.0625 pli
Polycarbonate 90° Peel, Conditioned for 3 days at 49°C; ASTM D3330
0.36156 kN/m
2.0625 pli
Finely Textured Powder Coating, 90° Peel, Conditioned for 3 days at 49°C; ASTM D3330
0.3725 kN/m
2.125 pli
Polypropylene, 90° Peel, Conditioned for 3 days at 49°C; ASTM D3330
0.38347 kN/m
2.1875 pli
LD Polyethylene, 90° Peel, Conditioned for 3 days at RT; ASTM D3330
0.40538 kN/m
2.3125 pli
HD Polyethylene, 90° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
0.4163 kN/m
2.375 pli
LD Polyethylene, 180° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
0.4163 kN/m
2.375 pli
LD Polyethylene, 90° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
0.4602 kN/m
2.625 pli
Finely Textured Powder Coating, 180° Peel, Initial, 10 min dwell at RT; ASTM D3330
0.4602 kN/m
2.625 pli
HD Polyethylene, 180° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
0.4602 kN/m
2.625 pli
Polypropylene, 90° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
0.482 kN/m
2.75 pli
Finely Textured Powder Coating, 180° Peel, Conditioned for 3 days at RT; ASTM D3330
0.49303 kN/m
2.8125 pli
Finely Textured Powder Coating, 180° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
0.5040 kN/m
2.875 pli
HD Polyethylene, 180° Peel, Initial, 10 min dwell at RT; ASTM D3330
0.5040 kN/m
2.875 pli
LD Polyethylene, 180° Peel, Initial, 10 min dwell at RT; ASTM D3330
0.526 kN/m
3.00 pli
HD Polyethylene, 180° Peel, Conditioned for 3 days at 49°C; ASTM D3330
0.526 kN/m
3.00 pli
Smooth Powder Coating, 90° Peel, Initial, 10 min dwell at RT; ASTM D3330
0.53686 kN/m
3.0625 pli
LD Polyethylene, 180° Peel, Conditioned for 3 days at RT; ASTM D3330
0.53686 kN/m
3.0625 pli
Finely Textured Powder Coating, 180° Peel, Conditioned for 3 days at 49°C; ASTM D3330
0.5478 kN/m
3.125 pli
Smooth Powder Coating, 90° Peel, Conditioned for 3 days at RT; ASTM D3330
0.55877 kN/m
3.1875 pli
HD Polyethylene, 180° Peel, Conditioned for 3 days at RT; ASTM D3330
0.614 kN/m
3.50 pli
Stainless Steel, 90° Peel, Initial, 10 min dwell at RT; ASTM D3330
0.62451 kN/m
3.5625 pli
Polycarbonate 90° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
0.6355 kN/m
3.625 pli
Smooth Powder Coating, 90° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
0.657 kN/m
3.75 pli
Smooth Powder Coating, 90° Peel, Conditioned for 3 days at 49°C; ASTM D3330
0.66833 kN/m
3.8125 pli
Polycarbonate 90° Peel, Initial, 10 min dwell at RT; ASTM D3330
0.69024 kN/m
3.9375 pli
Polycarbonate 180° Peel, Conditioned for 3 days at 49°C; ASTM D3330
0.71216 kN/m
4.0625 pli
Polypropylene, 180° Peel, Initial, 10 min dwell at RT; ASTM D3330
0.71216 kN/m
4.0625 pli
Glass, 90° Peel, Initial, 10 min dwell at RT; ASTM D3330
0.73407 kN/m
4.1875 pli
Polycarbonate 90° Peel, Conditioned for 3 days at RT; ASTM D3330
0.745 kN/m
4.25 pli
Polycarbonate 180° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
0.745 kN/m
4.25 pli
Polypropylene, 180° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
0.7669 kN/m
4.375 pli
Glass, 90° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
0.79981 kN/m
4.5625 pli
Smooth Powder Coating, 180° Peel, Initial, 10 min dwell at RT; ASTM D3330
0.8108 kN/m
4.625 pli
Polypropylene, 180° Peel, Conditioned for 3 days at RT; ASTM D3330
0.82172 kN/m
4.6875 pli
Glass, 90° Peel, Conditioned for 3 days at RT; ASTM D3330
0.84363 kN/m
4.8125 pli
Smooth Powder Coating, 180° Peel, Conditioned for 3 days at RT; ASTM D3330
0.84363 kN/m
4.8125 pli
Smooth Powder Coating, 180° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
0.8546 kN/m
4.875 pli
Stainless Steel, 90° Peel, Conditioned for 3 days at RT; ASTM D3330
0.86554 kN/m
4.9375 pli
Stainless Steel, 180° Peel, Initial, 10 min dwell at RT; ASTM D3330
0.86554 kN/m
4.9375 pli
Polypropylene, 180° Peel, Conditioned for 3 days at 49°C; ASTM D3330
0.877 kN/m
5.00 pli
Glass, 180° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
0.877 kN/m
5.00 pli
Stainless Steel, 90° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
0.88746 kN/m
5.0625 pli
Polycarbonate 180° Peel, Initial, 10 min dwell at RT; ASTM D3330
0.90937 kN/m
5.1875 pli
Glass, 180° Peel, Initial, 10 min dwell at RT; ASTM D3330
0.90937 kN/m
5.1875 pli
Smooth Powder Coating, 180° Peel, Conditioned for 3 days at 49°C; ASTM D3330
0.90937 kN/m
5.1875 pli
Glass, 90° Peel, Conditioned for 3 days at 49°C; ASTM D3330
0.9422 kN/m
5.375 pli
Polycarbonate 180° Peel, Conditioned for 3 days at RT; ASTM D3330
0.97511 kN/m
5.5625 pli
Glass, 180° Peel, Conditioned for 3 days at RT; ASTM D3330
1.0189 kN/m
5.8125 pli
Stainless Steel, 180° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
1.030 kN/m
5.875 pli
Stainless Steel, 90° Peel, Conditioned for 3 days at 49°C; ASTM D3330
1.05 kN/m
6.00 pli
Glass, 180° Peel, Conditioned for 3 days at 49°C; ASTM D3330
1.0628 kN/m
6.0625 pli
Stainless Steel, 180° Peel, Conditioned for 3 days at 49°C; ASTM D3330
15.8 kN/m
90.0 pli
Stainless Steel, 180° Peel, Conditioned for 3 days at RT; ASTM D3330