Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Arkema Group Pebax® 6333 SN 01 Polyether Block Amide (PEBA) (Dry)

Category Polymer , Thermoplastic , Elastomer, TPE , Polyether Block Amide (PEBA)
Manufacturer Arkema
Trade Name Pebax®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Arkema Group Pebax® 6333 SN 01 Polyether Block Amide (PEBA) (Dry).pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
POLYETHER BLOCK AMIDE (PEBA) hardness 63 shore D Non plasticized flexible Polyamide Outstanding mechanical properties at low temperature (-40°C) Applications: Sport (Football shoe sole, ski top layer...) Industrial (conveyor belts, transmission belts, electric coils...)ISO data provided by the manufacturer, Arkema.
Physical Properties Metric English Comments
Density 1.01 g/cc
0.0365 lb/in³
Water Absorption 1.1 %
1.1 %
Moisture Absorption at Equilibrium 0.60 %
0.60 %
Humidity Absorption
Melt Flow 8.0 g/10 min

@Load 1.00 kg,
Temperature 235 °C
8.0 g/10 min

@Load 2.20 lb,
Temperature 455 °F
Mechanical Properties Metric English Comments
Hardness, Shore D 63
63
Tensile Strength, Yield 19.0 MPa
2760 psi
50 mm/min
Elongation at Break >= 50 %
>= 50 %
Nominal Strain; 50 mm/min
Elongation at Yield 25 %
25 %
50 mm/min
Tensile Modulus 0.307 GPa
44.5 ksi
1 mm/min
Charpy Impact Unnotched NB
NB
NB
NB
Low Temp
Charpy Impact, Notched NB
NB
0.700 J/cm²

@Temperature -30.0 °C
3.33 ft-lb/in²

@Temperature -22.0 °F
Thermal Properties Metric English Comments
Melting Point 169 °C
336 °F
10°C/min
Flammability, UL94 HB

@Thickness 1.60 mm
HB

@Thickness 0.0630 in
Oxygen Index 20.2 %
20.2 %
Optical Properties Metric English Comments
Transmission, Visible 80 %
80 %
Mfr. reports 'Transparent' but doesn't quantify.
Electrical Properties Metric English Comments
Electrical Resistivity 9.33e+13 ohm-cm
9.33e+13 ohm-cm
Surface Resistance 2.67e+13 ohm
2.67e+13 ohm
Dielectric Strength 42.5 kV/mm
1080 kV/in
Dissipation Factor 0.00039

@Frequency 1e+6 Hz
0.00039

@Frequency 1e+6 Hz
0.000883

@Frequency 100 Hz
0.000883

@Frequency 100 Hz
Comparative Tracking Index 600 V
600 V
Users viewing this material also viewed the following: