Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

COI Ceramics Sylramic™ S200 Silicon Carbide Ceramic Matrix Composite, CG Nicalon

Category Ceramic , Carbide , Ceramic Matrix Composite
Manufacturer COI Ceramics
Trade Name Sylramic™
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF COI Ceramics Sylramic™ S200 Silicon Carbide Ceramic Matrix Composite, CG Nicalon.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Engineered ceramic composite structure.Reinforcing Fiber Flexibility: S400 - Carbon Preceramic Polymer Matrix Precursors: S400 - Crystalline (SiC + Si3N4) or SiCPhysical Attributes: Dense Matrix (
Mechanical Properties Metric English Comments
Tensile Strength 262 MPa

@Treatment Temp. 20.0 °C
38000 psi

@Treatment Temp. 68.0 °F
300 MPa

@Treatment Temp. 1000 °C
43500 psi

@Treatment Temp. 1830 °F
Tensile Stress 49.0 MPa

@Strain 0.0500 %,
Temperature 1204 °C
7110 psi

@Strain 0.0500 %,
Temperature 2199 °F
50.0 MPa

@Strain 0.0500 %,
Temperature 20.0 °C
7250 psi

@Strain 0.0500 %,
Temperature 68.0 °F
60.0 MPa

@Strain 0.0500 %,
Temperature 982 °C
8700 psi

@Strain 0.0500 %,
Temperature 1800 °F
90.3 MPa

@Strain 0.100 %,
Temperature 1204 °C
13100 psi

@Strain 0.100 %,
Temperature 2199 °F
95.1 MPa

@Strain 0.100 %,
Temperature 982 °C
13800 psi

@Strain 0.100 %,
Temperature 1800 °F
105 MPa

@Strain 0.100 %,
Temperature 20.0 °C
15200 psi

@Strain 0.100 %,
Temperature 68.0 °F
160 MPa

@Strain 0.300 %,
Temperature 1204 °C
23200 psi

@Strain 0.300 %,
Temperature 2199 °F
170 MPa

@Strain 0.300 %,
Temperature 982 °C
24700 psi

@Strain 0.300 %,
Temperature 1800 °F
185 MPa

@Strain 0.300 %,
Temperature 20.0 °C
26800 psi

@Strain 0.300 %,
Temperature 68.0 °F
225 MPa

@Strain 0.500 %,
Temperature 1204 °C
32600 psi

@Strain 0.500 %,
Temperature 2199 °F
240 MPa

@Strain 0.500 %,
Temperature 982 °C
34800 psi

@Strain 0.500 %,
Temperature 1800 °F
260 MPa

@Strain 0.500 %,
Temperature 20.0 °C
37700 psi

@Strain 0.500 %,
Temperature 68.0 °F
Tensile Strength, Yield 89.6 MPa

@Strain 0.0800 %,
Temperature 1000 °C
13000 psi

@Strain 0.0800 %,
Temperature 1830 °F
96.5 MPa

@Strain 0.0900 %,
Temperature 20.0 °C
14000 psi

@Strain 0.0900 %,
Temperature 68.0 °F
Elongation at Break 0.50 %

@Temperature 20.0 °C
0.50 %

@Temperature 68.0 °F
0.70 %

@Temperature 1000 °C
0.70 %

@Temperature 1830 °F
Elongation at Yield 0.08 %

@Temperature 1000 °C
0.08 %

@Temperature 1800 °F
Proportional Limit
0.09 %

@Temperature 20 °C
0.09 %

@Temperature 68 °F
Proportional Limit
Tensile Modulus 90.0 GPa

@Temperature 1000 °C
13100 ksi

@Temperature 1830 °F
96.0 GPa

@Temperature 20.0 °C
13900 ksi

@Temperature 68.0 °F
Flexural Strength 379 MPa

@Temperature 20.0 °C
55000 psi

@Temperature 68.0 °F
414 MPa

@Temperature 1000 °C
60000 psi

@Temperature 1830 °F
Compressive Strength 434 MPa

@Temperature 20.0 °C
62900 psi

@Temperature 68.0 °F
Shear Strength 24.0 MPa

@Temperature 1000 °C
3480 psi

@Temperature 1830 °F
38.0 MPa

@Temperature 20.0 °C
5510 psi

@Temperature 68.0 °F
Thermal Properties Metric English Comments
Thermal Conductivity 1.80 W/m-K

@Temperature 100 °C
12.5 BTU-in/hr-ft²-°F

@Temperature 212 °F
Thru-thickness
1.80 W/m-K

@Temperature 200 °C
12.5 BTU-in/hr-ft²-°F

@Temperature 392 °F
Thru-thickness
1.80 W/m-K

@Temperature 300 °C
12.5 BTU-in/hr-ft²-°F

@Temperature 572 °F
Thru-thickness
1.80 W/m-K

@Temperature 500 °C
12.5 BTU-in/hr-ft²-°F

@Temperature 932 °F
Thru-thickness
1.85 W/m-K

@Temperature 700 °C
12.8 BTU-in/hr-ft²-°F

@Temperature 1290 °F
Thru-thickness
1.85 W/m-K

@Temperature 500 °C
12.8 BTU-in/hr-ft²-°F

@Temperature 932 °F
Fill direction
1.85 W/m-K

@Temperature 500 °C
12.8 BTU-in/hr-ft²-°F

@Temperature 932 °F
Warp direction
1.90 W/m-K

@Temperature 300 °C
13.2 BTU-in/hr-ft²-°F

@Temperature 572 °F
Warp direction
1.90 W/m-K

@Temperature 900 °C
13.2 BTU-in/hr-ft²-°F

@Temperature 1650 °F
Thru-thickness
1.90 W/m-K

@Temperature 300 °C
13.2 BTU-in/hr-ft²-°F

@Temperature 572 °F
Fill direction
1.95 W/m-K

@Temperature 200 °C
13.5 BTU-in/hr-ft²-°F

@Temperature 392 °F
Warp direction
1.95 W/m-K

@Temperature 200 °C
13.5 BTU-in/hr-ft²-°F

@Temperature 392 °F
Fill direction
1.95 W/m-K

@Temperature 1000 °C
13.5 BTU-in/hr-ft²-°F

@Temperature 1830 °F
Thru-thickness
1.95 W/m-K

@Temperature 700 °C
13.5 BTU-in/hr-ft²-°F

@Temperature 1290 °F
Fill direction
1.95 W/m-K

@Temperature 700 °C
13.5 BTU-in/hr-ft²-°F

@Temperature 1290 °F
Warp direction
2.10 W/m-K

@Temperature 1000 °C
14.6 BTU-in/hr-ft²-°F

@Temperature 1830 °F
Warp direction
2.10 W/m-K

@Temperature 1000 °C
14.6 BTU-in/hr-ft²-°F

@Temperature 1830 °F
Fill direction
2.10 W/m-K

@Temperature 1200 °C
14.6 BTU-in/hr-ft²-°F

@Temperature 2190 °F
Thru-thickness
2.15 W/m-K

@Temperature 100 °C
14.9 BTU-in/hr-ft²-°F

@Temperature 212 °F
Warp direction
2.15 W/m-K

@Temperature 100 °C
14.9 BTU-in/hr-ft²-°F

@Temperature 212 °F
Fill direction
2.15 W/m-K

@Temperature 900 °C
14.9 BTU-in/hr-ft²-°F

@Temperature 1650 °F
Fill direction
2.15 W/m-K

@Temperature 900 °C
14.9 BTU-in/hr-ft²-°F

@Temperature 1650 °F
Warp direction
2.40 W/m-K

@Temperature 1200 °C
16.7 BTU-in/hr-ft²-°F

@Temperature 2190 °F
Warp direction
2.40 W/m-K

@Temperature 1200 °C
16.7 BTU-in/hr-ft²-°F

@Temperature 2190 °F
Fill direction
Users viewing this material also viewed the following: