| Category | Polymer , Thermoplastic , Acetal (POM) , Acetal Homopolymer, Unreinforced |
| Manufacturer | DuPont Performance Polymers |
| Trade Name | Delrin® |
| Port | Shanghai port,China |
| Trade Terms | FOB, CFR, CIF |
| Payment Terms | L/C, T/T, Western Union |
| Download PDF | DuPont Performance Polymers Delrin® 300PE BK602 Acetal (POM)
(Unverified Data**).pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.42 g/cc | 0.0513 lb/in³ | ISO 1183 |
| Viscosity | 102500 cP @Shear Rate 5000 1/s, Temperature 230 °C |
102500 cP @Shear Rate 5000 1/s, Temperature 446 °F |
ISO 11403-1 -2 |
| 104400 cP @Shear Rate 5000 1/s, Temperature 215 °C |
104400 cP @Shear Rate 5000 1/s, Temperature 419 °F |
ISO 11403-1 -2 | |
| 112500 cP @Shear Rate 5000 1/s, Temperature 200 °C |
112500 cP @Shear Rate 5000 1/s, Temperature 392 °F |
ISO 11403-1 -2 | |
| 369800 cP @Shear Rate 500 1/s, Temperature 230 °C |
369800 cP @Shear Rate 500 1/s, Temperature 446 °F |
ISO 11403-1 -2 | |
| 421400 cP @Shear Rate 500 1/s, Temperature 215 °C |
421400 cP @Shear Rate 500 1/s, Temperature 419 °F |
ISO 11403-1 -2 | |
| 452900 cP @Shear Rate 500 1/s, Temperature 200 °C |
452900 cP @Shear Rate 500 1/s, Temperature 392 °F |
ISO 11403-1 -2 | |
| Linear Mold Shrinkage, Flow | 0.020 cm/cm | 0.020 in/in | ISO 294-4 2577 |
| Linear Mold Shrinkage, Transverse | 0.018 cm/cm | 0.018 in/in | ISO 294-4 2577 |
| Melt Flow | 6.0 g/10 min @Load 2.16 kg, Temperature 190 °C |
6.0 g/10 min @Load 4.76 lb, Temperature 374 °F |
cm³/10min; ISO 1133 |
| 7.0 g/10 min @Load 2.16 kg, Temperature 190 °C |
7.0 g/10 min @Load 4.76 lb, Temperature 374 °F |
ISO 1133 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Rockwell M | 93 | 93 | ISO 2039-2 |
| Hardness, Rockwell R | 121 | 121 | ISO 2039-2 |
| Tensile Stress | 5.60 MPa @Strain 0.400 %, Temperature 90.0 °C |
812 psi @Strain 0.400 %, Temperature 194 °F |
ISO 11403-1 -2 |
| 19.1 MPa @Strain 1.80 %, Temperature 90.0 °C |
2770 psi @Strain 1.80 %, Temperature 194 °F |
ISO 11403-1 -2 | |
| 20.0 MPa @Strain 0.600 %, Temperature 23.0 °C |
2900 psi @Strain 0.600 %, Temperature 73.4 °F |
ISO 11403-1 -2 | |
| 26.8 MPa @Strain 3.20 %, Temperature 90.0 °C |
3890 psi @Strain 3.20 %, Temperature 194 °F |
ISO 11403-1 -2 | |
| 30.9 MPa @Strain 4.60 %, Temperature 90.0 °C |
4480 psi @Strain 4.60 %, Temperature 194 °F |
ISO 11403-1 -2 | |
| 34.1 MPa @Strain 0.800 %, Temperature -40.0 °C |
4950 psi @Strain 0.800 %, Temperature -40.0 °F |
ISO 11403-1 -2 | |
| 52.1 MPa @Strain 1.80 %, Temperature 0.000 °C |
7560 psi @Strain 1.80 %, Temperature 32.0 °F |
ISO 11403-1 -2 | |
| 54.3 MPa @Strain 2.60 %, Temperature 23.0 °C |
7880 psi @Strain 2.60 %, Temperature 73.4 °F |
ISO 11403-1 -2 | |
| 65.2 MPa @Strain 4.70 %, Temperature 23.0 °C |
9460 psi @Strain 4.70 %, Temperature 73.4 °F |
ISO 11403-1 -2 | |
| 68.6 MPa @Strain 7.00 %, Temperature 23.0 °C |
9950 psi @Strain 7.00 %, Temperature 73.4 °F |
ISO 11403-1 -2 | |
| 77.6 MPa @Strain 7.00 %, Temperature 0.000 °C |
11300 psi @Strain 7.00 %, Temperature 32.0 °F |
ISO 11403-1 -2 | |
| 79.1 MPa @Strain 12.0 %, Temperature 0.000 °C |
11500 psi @Strain 12.0 %, Temperature 32.0 °F |
ISO 11403-1 -2 | |
| 79.3 MPa @Strain 18.0 %, Temperature 0.000 °C |
11500 psi @Strain 18.0 %, Temperature 32.0 °F |
ISO 11403-1 -2 | |
| 87.1 MPa @Strain 3.40 %, Temperature -40.0 °C |
12600 psi @Strain 3.40 %, Temperature -40.0 °F |
ISO 11403-1 -2 | |
| 96.3 MPa @Strain 6.00 %, Temperature -40.0 °C |
14000 psi @Strain 6.00 %, Temperature -40.0 °F |
ISO 11403-1 -2 | |
| 98.2 MPa @Strain 9.00 %, Temperature -40.0 °C |
14200 psi @Strain 9.00 %, Temperature -40.0 °F |
ISO 11403-1 -2 | |
| Tensile Strength, Yield | 72.5 MPa | 10500 psi | ISO 527-1/-2 |
| Elongation at Break | 35 % | 35 % | Nominal; ISO 527-1/-2 |
| Elongation at Yield | 16 % | 16 % | ISO 527-1/-2 |
| Tensile Modulus | 3.30 GPa | 479 ksi | ISO 527-1/-2 |
| Flexural Strength | 84.0 MPa @Strain 3.50 % |
12200 psi @Strain 3.50 % |
ISO 178 |
| Flexural Modulus | 3.10 GPa | 450 ksi | ISO 178 |
| Secant Modulus | 0.548 GPa @Strain 12.8 %, Temperature 23.0 °C |
79.4 ksi @Strain 12.8 %, Temperature 73.4 °F |
ISO 11403-1 -2 |
| 0.566 GPa @Strain 14.0 %, Temperature 0.000 °C |
82.2 ksi @Strain 14.0 %, Temperature 32.0 °F |
ISO 11403-1 -2 | |
| 0.660 GPa @Strain 15.0 %, Temperature -40.0 °C |
95.7 ksi @Strain 15.0 %, Temperature -40.0 °F |
ISO 11403-1 -2 | |
| 0.774 GPa @Strain 9.00 %, Temperature 23.0 °C |
112 ksi @Strain 9.00 %, Temperature 73.4 °F |
ISO 11403-1 -2 | |
| 0.895 GPa @Strain 11.0 %, Temperature -40.0 °C |
130 ksi @Strain 11.0 %, Temperature -40.0 °F |
ISO 11403-1 -2 | |
| 1.11 GPa @Strain 7.00 %, Temperature 0.000 °C |
161 ksi @Strain 7.00 %, Temperature 32.0 °F |
ISO 11403-1 -2 | |
| 1.32 GPa @Strain 5.00 %, Temperature 23.0 °C |
191 ksi @Strain 5.00 %, Temperature 73.4 °F |
ISO 11403-1 -2 | |
| 1.39 GPa @Strain 7.00 %, Temperature -40.0 °C |
201 ksi @Strain 7.00 %, Temperature -40.0 °F |
ISO 11403-1 -2 | |
| 2.09 GPa @Strain 2.60 %, Temperature 23.0 °C |
303 ksi @Strain 2.60 %, Temperature 73.4 °F |
ISO 11403-1 -2 | |
| 2.56 GPa @Strain 3.40 %, Temperature -40.0 °C |
372 ksi @Strain 3.40 %, Temperature -40.0 °F |
ISO 11403-1 -2 | |
| 2.89 GPa @Strain 1.80 %, Temperature 0.000 °C |
420 ksi @Strain 1.80 %, Temperature 32.0 °F |
ISO 11403-1 -2 | |
| 3.33 GPa @Strain 0.600 %, Temperature 23.0 °C |
483 ksi @Strain 0.600 %, Temperature 73.4 °F |
ISO 11403-1 -2 | |
| 4.2625 GPa @Strain 0.800 %, Temperature -40.0 °C |
618.23 ksi @Strain 0.800 %, Temperature -40.0 °F |
ISO 11403-1 -2 | |
| Charpy Impact Unnotched | 27.5 J/cm² | 131 ft-lb/in² | ISO 179/1eU |
| 22.5 J/cm² @Temperature -30.0 °C |
107 ft-lb/in² @Temperature -22.0 °F |
ISO 179/1eU | |
| Charpy Impact, Notched | 1.00 J/cm² | 4.76 ft-lb/in² | ISO 179/1eA |
| 1.00 J/cm² @Temperature -30.0 °C |
4.76 ft-lb/in² @Temperature -22.0 °F |
ISO 179/1eA |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| Melting Point | 178 °C | 352 °F | 10°C/min; ISO 11357-1/-3 |
| Deflection Temperature at 1.8 MPa (264 psi) | 99.0 °C | 210 °F | ISO 75-1/-2 |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Volume Resistivity | >= 1.00e+15 ohm-cm | >= 1.00e+15 ohm-cm | IEC 60093 |
| Surface Resistance | 3.00e+14 ohm | 3.00e+14 ohm | IEC 60093 |
| Dielectric Constant | 3.9 @Frequency 100 Hz |
3.9 @Frequency 100 Hz |
IEC 60250 |
| 3.9 @Frequency 1.00e+6 Hz |
3.9 @Frequency 1.00e+6 Hz |
IEC 60250 | |
| Dielectric Strength | 43.0 kV/mm | 1090 kV/in | IEC 60243-1 |
| Dissipation Factor | 0.0010 @Frequency 100 Hz |
0.0010 @Frequency 100 Hz |
IEC 60250 |
| 0.0055 @Frequency 1.00e+6 Hz |
0.0055 @Frequency 1.00e+6 Hz |
IEC 60250 | |
| Comparative Tracking Index | 600 V | 600 V | IEC 60112 |
| Descriptive Properties | Value | Comments |
|---|---|---|
| Additives | Release agent | |
| Delivery Form | Pellets | |
| Emissions | <2 mg/kg | VDA 275 |
| Part Marking Code | >POM< | ISO 11469 |
| Processing | Injection Moulding | |
| Regional Availability | Asia Pacific | |
| Europe | ||
| Global | ||
| Near East/Africa | ||
| North America | ||
| South and Central America | ||
| Resin Identification | POM | ISO 1043 |