Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Kennametal Stellite Stellite® 12

Category Metal , Nonferrous Metal , Cobalt Alloy , Superalloy
Manufacturer Kennametal Stellite
Trade Name Stellite®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Kennametal Stellite Stellite® 12.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Satisfactory finishing results can be obtained using carbide tipped tools. Applications include cutting plastics, rubber, paper, carpet, and wood; saw teeth, trimmer knives, carpet knives, ledger blades, rotary slitters, grid nozzles, burner tips, guide rolls, sleeves, bushings, and for protecting bearing surfaces, screw flights, and veneer pressure bars. Data provided by the manufacturer, Deloro Stellite, Inc.Product of former Deloro Stellite Inc.
Physical Properties Metric English Comments
Density 8.52 g/cc
0.308 lb/in³
Mechanical Properties Metric English Comments
Hardness, Brinell 463
463
Converted from Rockwell C hardness.
Hardness, Rockwell A 75
75
Converted from Rockwell C hardness.
Hardness, Rockwell C 43 - 55
43 - 55
Hardness, Vickers 496
496
Converted from Rockwell C hardness.
Tensile Strength, Ultimate 690 MPa
100000 psi
(Tensile Yield Strength near U.T.S.)
Elongation at Break <= 1.0 %
<= 1.0 %
Modulus of Elasticity 226 GPa
32800 ksi
Ultimate Compressive Strength 1331 MPa
193000 psi
Izod Impact Unnotched 9.50 J
7.01 ft-lb
Thermal Properties Metric English Comments
CTE, linear 11.9 µm/m-°C

@Temperature 0.000 - 100 °C
6.61 µin/in-°F

@Temperature 32.0 - 212 °F
12.9 µm/m-°C

@Temperature 0.000 - 300 °C
7.17 µin/in-°F

@Temperature 32.0 - 572 °F
13.8 µm/m-°C

@Temperature 0.000 - 500 °C
7.67 µin/in-°F

@Temperature 32.0 - 932 °F
14.1 µm/m-°C

@Temperature 0.000 - 600 °C
7.83 µin/in-°F

@Temperature 32.0 - 1110 °F
14.4 µm/m-°C

@Temperature 0.000 - 700 °C
8.00 µin/in-°F

@Temperature 32.0 - 1290 °F
15.2 µm/m-°C

@Temperature 0.000 - 800 °C
8.44 µin/in-°F

@Temperature 32.0 - 1470 °F
15.2 µm/m-°C

@Temperature 0.000 - 900 °C
8.44 µin/in-°F

@Temperature 32.0 - 1650 °F
15.8 µm/m-°C

@Temperature 0.000 - 1000 °C
8.78 µin/in-°F

@Temperature 32.0 - 1830 °F
Thermal Conductivity 14.7 W/m-K
102 BTU-in/hr-ft²-°F
Melting Point 1255 - 1341 °C
2291 - 2446 °F
Solidus 1255 °C
2291 °F
Liquidus 1341 °C
2446 °F
Component Elements Properties Metric English Comments
Carbon, C 1.5 %
1.5 %
Chromium, Cr 29 %
29 %
Cobalt, Co 55.5 %
55.5 %
As remainder
Iron, Fe 2.0 %
2.0 %
Nickel, Ni 2.0 %
2.0 %
Silicon, Si 1.0 %
1.0 %
Tungsten, W 9.0 %
9.0 %
Copyright © lookpolymers.com All Rights Reserved