FeaturesDetermined for environment, where contact with water is possible, because the electric properties do not change by conditioning. Application - terminals, coil forms, guides in washing machines, tea-pots, dish-washers. Delivered in natural mode and in the full RAL colour scale. Modified homopolymer PP, retarded type with halogen flame retardant. Fulfills basic electric properties: flammability in accordance with UL 94 V0 and 960°C glow wire.Packaging, transport, stockingThe product is packed in hermetically closed thick-walled 25 kg PE bags, on a 1.000 kg palette coated in a stretch foil, in big bags with a thick PE foil fixed on a 1.000 kg palette, in paper octabins with a thick PE foil fixed on a 1.000 kg palette or in other packaging according to customer requirements. The transport is provided in closed-up vehicles where the material is protected against movement and mechanical damage. The product requires stocking in closed-up, dry places protected against sun and thermal radiation.Information Provided by Plastcom spol. s r.o.
Physical Properties Metric English Comments
Density 1.10 g/cc
0.0397 lb/in³
Linear Mold Shrinkage 0.0218 cm/cm
0.0218 in/in
Linear Mold Shrinkage, Transverse 0.0197 cm/cm
0.0197 in/in
Melt Flow 25 g/10 min

@Load 0.325 kg,
Temperature 270 °C
25 g/10 min

@Load 0.716 lb,
Temperature 518 °F
Mechanical Properties Metric English Comments
Tensile Strength at Break 30.0 MPa
4350 psi
Elongation at Break 10 %
10 %
Tensile Modulus 1.30 GPa
189 ksi
Flexural Strength 35.0 MPa
5080 psi
Flexural Modulus 1.30 GPa
189 ksi
Charpy Impact Unnotched 1.50 J/cm²

@Temperature -20.0 °C
7.14 ft-lb/in²

@Temperature -4.00 °F
9.00 J/cm²

@Temperature 23.0 °C
42.8 ft-lb/in²

@Temperature 73.4 °F
Charpy Impact, Notched 0.100 J/cm²

@Temperature -20.0 °C
0.476 ft-lb/in²

@Temperature -4.00 °F
0.300 J/cm²

@Temperature 23.0 °C
1.43 ft-lb/in²

@Temperature 73.4 °F
Thermal Properties Metric English Comments
Melting Point 160 °C
320 °F
Deflection Temperature at 1.8 MPa (264 psi) 90.0 °C
194 °F
Vicat Softening Point 150 °C
302 °F
B
Flammability, UL94 V-0
V-0
Glow Wire Test 960 °C
1760 °F
Electrical Properties Metric English Comments
Volume Resistivity 1.00e+14 ohm-cm
1.00e+14 ohm-cm
Surface Resistance 1.00e+16 ohm
1.00e+16 ohm
Dielectric Strength 26.0 kV/mm
660 kV/in
Comparative Tracking Index 450 V
450 V
Processing Properties Metric English Comments
Melt Temperature 200 - 250 °C
392 - 482 °F
Mold Temperature 30.0 - 50.0 °C
86.0 - 122 °F
Injection Pressure 50.0 - 80.0 MPa
7250 - 11600 psi