Quadrant EPP Ertalon® 4.6 PA 4.6, extruded (ISO Data)

Category Polymer , Thermoplastic , Nylon , Nylon 46 , Nylon 46, Unreinforced
Manufacturer Quadrant Engineering Plastics Products
Trade Name Ertalon®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Quadrant EPP Ertalon® 4.6 PA 4.6, extruded (ISO Data).pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Compared with conventional nylons, Ertalon 4.6 features a better retention of stiffness and creep resistance over a wide range of temperatures as well as superior heat ageing resistance. Therefore, applications for Ertalon 4.6 are situated in the “higher temperature area” (80 – 150 °C) where stiffness, creep resistance, heat ageing resistance, fatigue strength and wear resistance of PA 6, PA 66, POM and PET fall short. High mechanical strength, stiffness, hardness and toughness Good fatigue resistance High mechanical damping ability Good sliding properties Excellent wear resistance Good electrical insulating properties Good resistance to high energy radiation (gamma- and X-rays) Good machinability
Physical Properties Metric English Comments
Density 1.19 g/cc
0.0430 lb/in³
ISO 1183-1
Moisture Absorption at Equilibrium 2.8 %
2.8 %
50% RH
Water Absorption at Saturation 9.5 %
9.5 %
Mechanical Properties Metric English Comments
Hardness, Rockwell M 92
92
ISO 2039-2
Hardness, Shore D 80
80
Ball Indentation Hardness 165 MPa
23900 psi
ISO 2039-1
Tensile Strength 105 MPa
15200 psi
at Yield; ISO 527-1/-2
Elongation at Break 25 %
25 %
ISO 527-1/-2
Elongation at Yield 18 %
18 %
ISO 527-1/-2
Tensile Modulus 3.40 GPa
493 ksi
ISO 527-1/-2
Flexural Strength 138 MPa
20000 psi
Flexural Modulus 3.23 GPa
468 ksi
Compressive Strength 31.0 MPa

@Strain 1 %
4500 psi

@Strain 1 %
ISO 604
60.0 MPa

@Strain 2 %
8700 psi

@Strain 2 %
ISO 604
102 MPa

@Strain 5 %
14800 psi

@Strain 5 %
ISO 604
K Factor (ISO) 18 µm/km
18 µm/km
Charpy Impact Unnotched NB
NB
ISO 179-1/1eU
Charpy Impact, Notched 0.800 J/cm²
3.81 ft-lb/in²
ISO 179-1/1eA
Coefficient of Friction, Dynamic 0.40 - 0.60
0.40 - 0.60
Limiting Pressure Velocity 0.100 MPa-m/sec
2860 psi-ft/min
at 1 m/s unlubricated
0.160 MPa-m/sec
4570 psi-ft/min
at 0.1 m/s unlubricated
Thermal Properties Metric English Comments
CTE, linear 90.0 µm/m-°C

@Temperature 23.0 - 100 °C
50.0 µin/in-°F

@Temperature 73.4 - 212 °F
Thermal Conductivity 0.300 W/m-K
2.08 BTU-in/hr-ft²-°F
Melting Point 290 °C
554 °F
DSC, 10°C/min.; ISO 11357-1/-3
Maximum Service Temperature, Air 130 °C
266 °F
Continuous; 20,000 h
150 °C
302 °F
Continuous; 5,000 h
Deflection Temperature at 1.8 MPa (264 psi) 160 °C
320 °F
ISO 75-1/-2
Flammability, UL94 HB
HB
Oxygen Index 24 %
24 %
ISO 4589-1/-2
Electrical Properties Metric English Comments
Volume Resistivity >= 1.0e+14 ohm-cm
>= 1.0e+14 ohm-cm
IEC 60093
Surface Resistivity per Square >= 1.0e+13 ohm
>= 1.0e+13 ohm
IEC 60093
Dielectric Constant 3.8

@Frequency >=100000 Hz
3.8

@Frequency >=100000 Hz
IEC 60250
Dielectric Strength 25.0 kV/mm
635 kV/in
Dissipation Factor 0.0090

@Frequency 100000 Hz
0.0090

@Frequency 100000 Hz
IEC 60250
Comparative Tracking Index 400 V
400 V
IEC 60112
Compliance Properties Metric English Comments
3A-Dairy No
No
European Food 1935/2004 No
No
FDA No
No
USP Class VI No
No
Chemical Resistance Properties Metric English Comments
Acids, Strong (pH 1-3) Unacceptable
Unacceptable
Acids, Weak Limited
Limited
Alcohols Limited
Limited
Alkalies, Strong (pH 11-14) Unacceptable
Unacceptable
Alkalies, Weak Limited
Limited
Chlorinated Solvents Limited
Limited
Continuous Sunlight Limited
Limited
Hot Water / Steam Limited
Limited
Hydrocarbons - Aliphatic Acceptable
Acceptable
Hydrocarbons - Aromatic Acceptable
Acceptable
Inorganic Salt Solutions Acceptable
Acceptable
Ketones, Esters Acceptable
Acceptable