Material Notes:
TRA-CAST 3156 is an easy-to-use, low cost, versatile epoxy resin and hardener system developed for general purpose casting applications. It develops excellent adhesion to most metals, plastics, and ceramics, and is recommended for electrical and structural potting and encapsulating applications where the combination of good mechanical, thermal, electrical and room temperature cure properties are required. Fully cured TRA-CAST 3156 is a strong, tough, electrical insulator with high heat stability and a low thermal coefficient of expansion that provides successful performance over a wide temperature range. It is resistant to industrial environments that include water, weather, galvanic action, petroleum fuels, lubricants and solvents, gases and vapors, many mild acids and alkalis.Information provided by Tra-Con Inc.
Physical Properties Metric English Comments
Specific Gravity 1.50 g/cc
1.50 g/cc
Mixed
Volatile Organic Compounds (VOC) Content 4.45 g/l
4.45 g/l
Water Absorption 0.50 %
0.50 %
After 24 hours
Viscosity 24500 cP

@Temperature 25.0 °C
24500 cP

@Temperature 77.0 °F
Mixed (sp #7, 10 rpm)
Mechanical Properties Metric English Comments
Hardness, Shore D 87
87
Tensile Strength, Yield 84.8 MPa
12300 psi
Compressive Strength 112 MPa
16200 psi
Adhesive Bond Strength 8.62 MPa
1250 psi
Lap shear, alum to alum, 24 hrs @ 25°C
9.31 MPa
1350 psi
Lap shear, alum to alum, 4 hrs @ 25°C + 2 hrs @ 65°C
Thermal Properties Metric English Comments
CTE, linear 87.1 µm/m-°C
48.4 µin/in-°F
Below Tg
210 µm/m-°C
117 µin/in-°F
Above Tg
Maximum Service Temperature, Air 155 °C
311 °F
Minimum Service Temperature, Air -60.0 °C
-76.0 °F
Glass Transition Temp, Tg 82.0 °C
180 °F
Ultimate Tg
Electrical Properties Metric English Comments
Volume Resistivity 6.50e+15 ohm-cm
6.50e+15 ohm-cm
Dielectric Constant 3.9

@Frequency 1e+6 Hz
3.9

@Frequency 1e+6 Hz
4.6

@Frequency 1000 Hz
4.6

@Frequency 1000 Hz
Dielectric Strength 17.7 kV/mm
450 kV/in
Dissipation Factor 0.010

@Frequency 1000 Hz
0.010

@Frequency 1000 Hz
0.020

@Frequency 1e+6 Hz
0.020

@Frequency 1e+6 Hz
Processing Properties Metric English Comments
Cure Time 360 min
6.00 hour
4 hrs @ 25°C + 2 hrs @ 65°C
1440 min

@Temperature 25.0 °C
24.0 hour

@Temperature 77.0 °F
Pot Life 25 min
25 min
25 grams
45 min
45 min
100 grams
Descriptive Properties Value Comments
Color Black
Heat Distortion Temperature °C 105
Working Life hours 1.5
100 grams
Users viewing this material also viewed the following: