| Category | Polymer , Thermoplastic , Nylon , Nylon 6 , Nylon 6, 30% Mineral Filled |
| Manufacturer | Addiplast |
| Trade Name | Addinyl |
| Port | Shanghai port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | Addiplast Addinyl B2H M30 Flame Retardant Nylon 6, 30% Mineral Filled.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.62 g/cc | 0.0585 lb/in³ | ISO 1183/A |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Shore D | 80 | 80 | Conditioned; ISO 868 |
| 85 | 85 | ISO 868 | |
| Tensile Strength at Break | 40.0 MPa | 5800 psi | Conditioned; ISO R 527 |
| 70.0 MPa | 10200 psi | ISO R 527 | |
| Elongation at Break | 5.0 % | 5.0 % | ISO R 527 |
| 10 % | 10 % | Conditioned; ISO R 527 | |
| Modulus of Elasticity | 3.50 GPa | 508 ksi | Conditioned; ISO 178 |
| 7.00 GPa | 1020 ksi | ISO 178 | |
| Izod Impact, Notched (ISO) | 4.00 kJ/m² | 1.90 ft-lb/in² | ISO 180/1A |
| 7.00 kJ/m² | 3.33 ft-lb/in² | Conditioned; ISO 180/1A | |
| Charpy Impact Unnotched | 3.00 J/cm² | 14.3 ft-lb/in² | ISO 179/IeU |
| 5.00 J/cm² | 23.8 ft-lb/in² | Conditioned; ISO 179/IeU | |
| Charpy Impact, Notched | 0.400 J/cm² | 1.90 ft-lb/in² | ISO 179/IeA |
| 0.600 J/cm² | 2.86 ft-lb/in² | Conditioned; ISO 179/IeA |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| Melting Point | 220 °C | 428 °F | ISO 3146/C2 |
| Deflection Temperature at 1.8 MPa (264 psi) | 150 °C | 302 °F | ISO 75-2/AF |
| Flammability, UL94 | V-0 @Thickness 1.60 mm |
V-0 @Thickness 0.0630 in |
|
| Oxygen Index | 32 % | 32 % | ISO 4589 |
| Glow Wire Test | 960 °C | 1760 °F | CEI 60695/2/1 |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Volume Resistivity | 1.00e+12 ohm-cm | 1.00e+12 ohm-cm | Conditioned; CEI 60093 |
| 1.00e+15 ohm-cm | 1.00e+15 ohm-cm | CEI 60093 | |
| Surface Resistance | 1.00e+14 ohm | 1.00e+14 ohm | CEI 60093 |
| Comparative Tracking Index | 350 V | 350 V | CEI 60112/Solution A |