| Category | Polymer , Thermoplastic , Nylon , Nylon 66 , Nylon 66, 30% Glass Fiber Filled |
| Manufacturer | DuPont Performance Polymers |
| Trade Name | Zytel® |
| Port | Shanghai port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | DuPont Performance Polymers Zytel® 70G30HSLR NC010 Nylon 66
(Unverified Data**).pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.37 g/cc | 0.0495 lb/in³ | DAM; ISO 1183 |
| Filler Content | 30 % | 30 % | DAM |
| Water Absorption | 1.9 % @Temperature 23.0 °C |
1.9 % @Temperature 73.4 °F |
Equilibrium 50%RH; DAM; ISO 62, Similar to |
| 6.0 % @Temperature 23.0 °C |
6.0 % @Temperature 73.4 °F |
Saturation, immersed; DAM; ISO 62, Similar to | |
| Viscosity | 58000 cP @Shear Rate 7000 1/s, Temperature 305 °C |
58000 cP @Shear Rate 7000 1/s, Temperature 581 °F |
DAM; ISO 11443 |
| 69000 cP @Shear Rate 5000 1/s, Temperature 305 °C |
69000 cP @Shear Rate 5000 1/s, Temperature 581 °F |
DAM; ISO 11443 | |
| 73000 cP @Shear Rate 7000 1/s, Temperature 295 °C |
73000 cP @Shear Rate 7000 1/s, Temperature 563 °F |
DAM; ISO 11443 | |
| 86000 cP @Shear Rate 5000 1/s, Temperature 295 °C |
86000 cP @Shear Rate 5000 1/s, Temperature 563 °F |
DAM; ISO 11443 | |
| 107000 cP @Shear Rate 2000 1/s, Temperature 305 °C |
107000 cP @Shear Rate 2000 1/s, Temperature 581 °F |
DAM; ISO 11443 | |
| 116000 cP @Shear Rate 7000 1/s, Temperature 275 °C |
116000 cP @Shear Rate 7000 1/s, Temperature 527 °F |
DAM; ISO 11443 | |
| 134000 cP @Shear Rate 2000 1/s, Temperature 295 °C |
134000 cP @Shear Rate 2000 1/s, Temperature 563 °F |
DAM; ISO 11443 | |
| 137000 cP @Shear Rate 5000 1/s, Temperature 275 °C |
137000 cP @Shear Rate 5000 1/s, Temperature 527 °F |
DAM; ISO 11443 | |
| 147000 cP @Shear Rate 1000 1/s, Temperature 305 °C |
147000 cP @Shear Rate 1000 1/s, Temperature 581 °F |
DAM; ISO 11443 | |
| 171000 cP @Shear Rate 700 1/s, Temperature 305 °C |
171000 cP @Shear Rate 700 1/s, Temperature 581 °F |
DAM; ISO 11443 | |
| 185000 cP @Shear Rate 1000 1/s, Temperature 295 °C |
185000 cP @Shear Rate 1000 1/s, Temperature 563 °F |
DAM; ISO 11443 | |
| 196000 cP @Shear Rate 500 1/s, Temperature 305 °C |
196000 cP @Shear Rate 500 1/s, Temperature 581 °F |
DAM; ISO 11443 | |
| 215000 cP @Shear Rate 700 1/s, Temperature 295 °C |
215000 cP @Shear Rate 700 1/s, Temperature 563 °F |
DAM; ISO 11443 | |
| 216000 cP @Shear Rate 2000 1/s, Temperature 275 °C |
216000 cP @Shear Rate 2000 1/s, Temperature 527 °F |
DAM; ISO 11443 | |
| 248000 cP @Shear Rate 500 1/s, Temperature 295 °C |
248000 cP @Shear Rate 500 1/s, Temperature 563 °F |
DAM; ISO 11443 | |
| 299000 cP @Shear Rate 1000 1/s, Temperature 275 °C |
299000 cP @Shear Rate 1000 1/s, Temperature 527 °F |
DAM; ISO 11443 | |
| 350000 cP @Shear Rate 700 1/s, Temperature 275 °C |
350000 cP @Shear Rate 700 1/s, Temperature 527 °F |
DAM; ISO 11443 | |
| 404000 cP @Shear Rate 500 1/s, Temperature 275 °C |
404000 cP @Shear Rate 500 1/s, Temperature 527 °F |
DAM; ISO 11443 | |
| Linear Mold Shrinkage, Flow | 0.0030 cm/cm @Thickness 2.00 mm |
0.0030 in/in @Thickness 0.0787 in |
DAM; ISO 294-4 |
| Linear Mold Shrinkage, Transverse | 0.011 cm/cm @Thickness 2.00 mm |
0.011 in/in @Thickness 0.0787 in |
DAM; ISO 294-4 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 130 MPa @Temperature 23.0 °C |
18900 psi @Temperature 73.4 °F |
50%RH; ISO 527 |
| 195 MPa @Temperature 23.0 °C |
28300 psi @Temperature 73.4 °F |
DAM; ISO 527 | |
| Elongation at Break | 3.3 % @Temperature 23.0 °C |
3.3 % @Temperature 73.4 °F |
DAM; ISO 527 |
| 5.0 % @Temperature 23.0 °C |
5.0 % @Temperature 73.4 °F |
50%RH; ISO 527 | |
| Tensile Modulus | 7.20 GPa @Temperature 23.0 °C |
1040 ksi @Temperature 73.4 °F |
50%RH; ISO 527 |
| 10.0 GPa @Temperature 23.0 °C |
1450 ksi @Temperature 73.4 °F |
DAM; ISO 527 | |
| Izod Impact, Notched (ISO) | 10.0 kJ/m² @Temperature -30.0 °C |
4.76 ft-lb/in² @Temperature -22.0 °F |
50%RH; ISO 180/1A |
| 12.0 kJ/m² @Temperature -30.0 °C |
5.71 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 180/1A | |
| 12.0 kJ/m² @Temperature 23.0 °C |
5.71 ft-lb/in² @Temperature 73.4 °F |
DAM; ISO 180/1A | |
| 14.0 kJ/m² @Temperature 23.0 °C |
6.66 ft-lb/in² @Temperature 73.4 °F |
50%RH; ISO 180/1A | |
| Charpy Impact Unnotched | 7.00 J/cm² @Temperature -30.0 °C |
33.3 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 179/1eU |
| 7.20 J/cm² @Temperature -30.0 °C |
34.3 ft-lb/in² @Temperature -22.0 °F |
50%RH; ISO 179/1eU | |
| 8.20 J/cm² @Temperature 23.0 °C |
39.0 ft-lb/in² @Temperature 73.4 °F |
DAM; ISO 179/1eU | |
| 9.20 J/cm² @Temperature 23.0 °C |
43.8 ft-lb/in² @Temperature 73.4 °F |
50%RH; ISO 179/1eU | |
| Charpy Impact, Notched | 1.00 J/cm² @Temperature -30.0 °C |
4.76 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 179/1eA |
| 1.00 J/cm² @Temperature -30.0 °C |
4.76 ft-lb/in² @Temperature -22.0 °F |
50%RH; ISO 179/1eA | |
| 1.30 J/cm² @Temperature 23.0 °C |
6.19 ft-lb/in² @Temperature 73.4 °F |
DAM; ISO 179/1eA | |
| 1.50 J/cm² @Temperature 23.0 °C |
7.14 ft-lb/in² @Temperature 73.4 °F |
50%RH; ISO 179/1eA | |
| Tensile Creep Modulus, 1 hour | 6800 MPa @Temperature 23.0 °C |
986000 psi @Temperature 73.4 °F |
50%RH; ISO 899 |
| 10.0 MPa @Strain 0.172 %, Temperature 100 °C |
1450 psi @Strain 0.172 %, Temperature 212 °F |
50%RH; 10h; Isochronous; ISO 899 | |
| 10.0 MPa @Strain 0.169 %, Temperature 80.0 °C |
1450 psi @Strain 0.169 %, Temperature 176 °F |
50%RH; 10h; Isochronous; ISO 899 | |
| 10.0 MPa @Strain 0.159 %, Temperature 80.0 °C |
1450 psi @Strain 0.159 %, Temperature 176 °F |
50%RH; 1h; Isochronous; ISO 899 | |
| 10.0 MPa @Strain 0.167 %, Temperature 100 °C |
1450 psi @Strain 0.167 %, Temperature 212 °F |
50%RH; 1h; Isochronous; ISO 899 | |
| 15.0 MPa @Strain 0.244 %, Temperature 80.0 °C |
2180 psi @Strain 0.244 %, Temperature 176 °F |
50%RH; 1h; Isochronous; ISO 899 | |
| 15.0 MPa @Strain 0.259 %, Temperature 80.0 °C |
2180 psi @Strain 0.259 %, Temperature 176 °F |
50%RH; 10h; Isochronous; ISO 899 | |
| 15.0 MPa @Strain 0.205 %, Temperature 23.0 °C |
2180 psi @Strain 0.205 %, Temperature 73.4 °F |
50%RH; 10h; Isochronous; ISO 899 | |
| 15.0 MPa @Strain 0.190 %, Temperature 23.0 °C |
2180 psi @Strain 0.190 %, Temperature 73.4 °F |
50%RH; 1h; Isochronous; ISO 899 | |
| 20.0 MPa @Strain 0.371 %, Temperature 100 °C |
2900 psi @Strain 0.371 %, Temperature 212 °F |
50%RH; 1h; Isochronous; ISO 899 | |
| 20.0 MPa @Strain 0.352 %, Temperature 80.0 °C |
2900 psi @Strain 0.352 %, Temperature 176 °F |
50%RH; 10h; Isochronous; ISO 899 | |
| 20.0 MPa @Strain 0.396 %, Temperature 100 °C |
2900 psi @Strain 0.396 %, Temperature 212 °F |
50%RH; 10h; Isochronous; ISO 899 | |
| 20.0 MPa @Strain 0.333 %, Temperature 80.0 °C |
2900 psi @Strain 0.333 %, Temperature 176 °F |
50%RH; 1h; Isochronous; ISO 899 | |
| 25.0 MPa @Strain 0.345 %, Temperature 23.0 °C |
3630 psi @Strain 0.345 %, Temperature 73.4 °F |
50%RH; 10h; Isochronous; ISO 899 | |
| 25.0 MPa @Strain 0.322 %, Temperature 23.0 °C |
3630 psi @Strain 0.322 %, Temperature 73.4 °F |
50%RH; 1h; Isochronous; ISO 899 | |
| 30.0 MPa @Strain 0.391 %, Temperature 23.0 °C |
4350 psi @Strain 0.391 %, Temperature 73.4 °F |
50%RH; 1h; Isochronous; ISO 899 | |
| 30.0 MPa @Strain 0.418 %, Temperature 23.0 °C |
4350 psi @Strain 0.418 %, Temperature 73.4 °F |
50%RH; 10h; Isochronous; ISO 899 | |
| 30.0 MPa @Strain 0.594 %, Temperature 100 °C |
4350 psi @Strain 0.594 %, Temperature 212 °F |
50%RH; 1h; Isochronous; ISO 899 | |
| 30.0 MPa @Strain 0.564 %, Temperature 80.0 °C |
4350 psi @Strain 0.564 %, Temperature 176 °F |
50%RH; 10h; Isochronous; ISO 899 | |
| 30.0 MPa @Strain 0.622 %, Temperature 100 °C |
4350 psi @Strain 0.622 %, Temperature 212 °F |
50%RH; 10h; Isochronous; ISO 899 | |
| 30.0 MPa @Strain 0.529 %, Temperature 80.0 °C |
4350 psi @Strain 0.529 %, Temperature 176 °F |
50%RH; 1h; Isochronous; ISO 899 | |
| 40.0 MPa @Strain 0.759 %, Temperature 80.0 °C |
5800 psi @Strain 0.759 %, Temperature 176 °F |
50%RH; 1h; Break; Isochronous; ISO 899 |