| Category | Polymer , Thermoplastic , Polyester, TP , Polybutylene Terephthalate (PBT) |
| Manufacturer | SABIC Innovative Plastics (GE Plastics) |
| Trade Name | Valox® |
| Port | Ningbo port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | SABIC Innovative Plastics Valox® V2105U PBT (Europe-Africa-Middle East).pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.28 g/cc | 1.28 g/cc | ASTM D792 |
| Density | 1.28 g/cc | 0.0462 lb/in³ | ISO 1183 |
| Moisture Absorption | 0.0800 % | 0.0800 % | 23°C / 50% RH; ISO 62 |
| Water Absorption at Saturation | 0.34 % | 0.34 % | ISO 62 |
| Linear Mold Shrinkage, Flow | 0.029 - 0.034 cm/cm @Thickness 3.20 mm |
0.029 - 0.034 in/in @Thickness 0.126 in |
SABIC Method |
| Linear Mold Shrinkage, Transverse | 0.025 - 0.030 cm/cm @Thickness 3.20 mm |
0.025 - 0.030 in/in @Thickness 0.126 in |
SABIC Method |
| Melt Flow | 9.5 g/10 min @Load 5.00 kg, Temperature 266 °C |
9.5 g/10 min @Load 11.0 lb, Temperature 511 °F |
ASTM D1238 |
| Melt Index of Compound | 8.0 g/10 min @Load 5.00 kg, Temperature 265 °C |
8.0 g/10 min @Load 11.0 lb, Temperature 509 °F |
MVR [cm^3/10 min]; ISO 1133 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 52.0 MPa | 7540 psi | 50 mm/min; ISO 527 |
| 58.0 MPa | 8410 psi | Type I, 50 mm/min; ASTM D638 | |
| Tensile Strength, Yield | 39.0 MPa | 5660 psi | Type I, 50 mm/min; ASTM D638 |
| 40.0 MPa | 5800 psi | 50 mm/min; ISO 527 | |
| Elongation at Break | 230 % | 230 % | 50 mm/min; ISO 527 |
| 300 % | 300 % | Type I, 50 mm/min; ASTM D638 | |
| Elongation at Yield | 6.0 % | 6.0 % | 50 mm/min; ISO 527 |
| 17 % | 17 % | Type I, 50 mm/min; ASTM D638 | |
| Tensile Modulus | 2.50 GPa | 363 ksi | 5 mm/min; ASTM D638 |
| 2.54 GPa | 368 ksi | 1 mm/min; ISO 527 | |
| Flexural Yield Strength | 62.0 MPa | 8990 psi | 2 mm/min; ISO 178 |
| 65.0 MPa | 9430 psi | 1.3 mm/min, 50 mm span; ASTM D790 | |
| Flexural Modulus | 1.87 GPa | 271 ksi | 2 mm/min; ISO 178 |
| 2.06 GPa | 299 ksi | 1.3 mm/min, 50 mm span; ASTM D790 | |
| Izod Impact, Notched | 11.6 J/cm | 21.7 ft-lb/in | ASTM D256 |
| 1.50 J/cm @Temperature -30.0 °C |
2.81 ft-lb/in @Temperature -22.0 °F |
ASTM D256 | |
| Izod Impact, Notched (ISO) | 98.0 kJ/m² | 46.6 ft-lb/in² | 80*10*4; ISO 180/1A |
| 15.0 kJ/m² @Temperature -30.0 °C |
7.14 ft-lb/in² @Temperature -22.0 °F |
80*10*4; ISO 180/1A | |
| Charpy Impact, Notched | 9.00 J/cm² | 42.8 ft-lb/in² | Edgew 80*10*4 sp=62mm; ISO 179/1eA |
| Dart Drop, Total Energy | 63.0 J @Temperature 23.0 °C |
46.5 ft-lb @Temperature 73.4 °F |
ASTM D3763 |
| 75.0 J @Temperature -40.0 °C |
55.3 ft-lb @Temperature -40.0 °F |
ASTM D3763 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 80.0 µm/m-°C @Temperature -40.0 - 40.0 °C |
44.4 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 |
| 80.0 µm/m-°C @Temperature -40.0 - 40.0 °C |
44.4 µin/in-°F @Temperature -40.0 - 104 °F |
ISO 11359-2 | |
| CTE, linear, Transverse to Flow | 120 µm/m-°C @Temperature -40.0 - 40.0 °C |
66.7 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 |
| 120 µm/m-°C @Temperature -40.0 - 40.0 °C |
66.7 µin/in-°F @Temperature -40.0 - 104 °F |
ISO 11359-2 | |
| Deflection Temperature at 1.8 MPa (264 psi) | 47.0 °C | 117 °F | Flatw 80*10*4 sp=64mm; ISO 75/Af |
| 49.0 °C @Thickness 3.20 mm |
120 °F @Thickness 0.126 in |
unannealed; ASTM D648 | |
| Vicat Softening Point | 158 °C | 316 °F | Rate B/50; ASTM D1525 |
| 158 °C | 316 °F | Rate B/50; ISO 306 | |
| 158 °C | 316 °F | Rate B/120; ISO 306 |