Material Notes:
The use of this highly temperature resistant polyamide enables reliable operation up to a constant service temperature of 155°C . The material retains its rigidity and creep strength over the entire temperature range far better than other Murylon® types.Special Properties:• Highly wear-resistant and good slide properties, especially at high temperatures• Good resistance to thermal aging• High creep resistanceInformation provided by Murtfeldt Kunststoffe GmbH & Co. KG.
Physical Properties Metric English Comments
Density 1.18 g/cc
0.0426 lb/in³
ISO 1183-1
Moisture Absorption at Equilibrium 2.8 %

@Temperature 23.0 °C
2.8 %

@Temperature 73.4 °F
50% RH
Water Absorption at Saturation 9.5 %

@Temperature 23.0 °C
9.5 %

@Temperature 73.4 °F
Mechanical Properties Metric English Comments
Hardness, Rockwell M 92
92
ISO 2039-2
Hardness, Shore D 80
80
DIN 53505
Ball Indentation Hardness 165 MPa
23900 psi
ISO 2039-1
Tensile Strength, Yield 55.0 MPa
7980 psi
50% RH; ISO 527-1/-2
105 MPa
15200 psi
dry; ISO 527-1/-2
Elongation at Break 25 %
25 %
dry; ISO 527-1/-2
>= 100 %
>= 100 %
50% RH; ISO 527-1/-2
Creep Strength 7.50 MPa
1090 psi
stress leading to 1% elongation; 50% RH; ISO 899-1
22.0 MPa
3190 psi
stress leading to 1% elongation; dry; ISO 899-1
Modulus of Elasticity 1.35 GPa
196 ksi
50% RH
3.40 GPa
493 ksi
dry
Compressive Yield Strength 23.0 MPa

@Strain 1.00 %
3340 psi

@Strain 1.00 %
dry; ISO 604
45.0 MPa

@Strain 2.00 %
6530 psi

@Strain 2.00 %
dry; ISO 604
94.0 MPa

@Strain 5.00 %
13600 psi

@Strain 5.00 %
dry; ISO 604
Charpy Impact Unnotched NB
NB
ISO 179-1/1eU
NB
NB
ISO 179
Charpy Impact, Notched 0.800 J/cm²
3.81 ft-lb/in²
ISO 179-1/1eA
Coefficient of Friction, Dynamic 0.34
0.34
Thermal Properties Metric English Comments
CTE, linear 80.0 µm/m-°C

@Temperature 23.0 - 60.0 °C
44.4 µin/in-°F

@Temperature 73.4 - 140 °F
90.0 µm/m-°C

@Temperature 23.0 - 100 °C
50.0 µin/in-°F

@Temperature 73.4 - 212 °F
Melting Point 290 °C
554 °F
ISO 11357-1
Maximum Service Temperature, Air 130 °C

@Time 7.20e+7 sec
266 °F

@Time 20000 hour
150 °C

@Time 1.80e+7 sec
302 °F

@Time 5000 hour
200 °C

@Time <=86400 sec
392 °F

@Time <=24.0 hour
Minimum Service Temperature, Air -40.0 °C
-40.0 °F
Glass Transition Temp, Tg 80.0 °C
176 °F
ISO 11357-1
Flammability, UL94 HB
HB
Electrical Properties Metric English Comments
Electrical Resistivity >= 1.00e+12 ohm-cm
>= 1.00e+12 ohm-cm
50% RH; IEC 60093
>= 1.00e+14 ohm-cm
>= 1.00e+14 ohm-cm
dry; IEC 60093
Surface Resistance >= 1.00e+12 ohm
>= 1.00e+12 ohm
50% RH; IEC 60093
>= 1.00e+13 ohm
>= 1.00e+13 ohm
dry; IEC 60093
Dielectric Constant 3.4

@Frequency 1.00e+6 Hz
3.4

@Frequency 1.00e+6 Hz
dry; IEC 60250
3.5

@Frequency 100 Hz
3.5

@Frequency 100 Hz
dry; IEC 60250
3.8

@Frequency 1.00e+6 Hz
3.8

@Frequency 1.00e+6 Hz
50% RH; IEC 60250
7.4

@Frequency 100 Hz
7.4

@Frequency 100 Hz
50% RH; IEC 60250
Dielectric Strength 15.0 kV/mm
381 kV/in
50% RH; IEC 60243-1
25.0 kV/mm
635 kV/in
dry; IEC 60243-1
Dielectric Loss Index 0.0090

@Frequency 100 Hz
0.0090

@Frequency 100 Hz
dry; IEC 60250
0.019

@Frequency 1.00e+6 Hz
0.019

@Frequency 1.00e+6 Hz
dry; IEC 60250
0.060

@Frequency 1.00e+6 Hz
0.060

@Frequency 1.00e+6 Hz
50% RH; IEC 60250
0.13

@Frequency 100 Hz
0.13

@Frequency 100 Hz
50% RH; IEC 60250
Compliance Properties Metric English Comments
FDA Yes
Yes
Descriptive Properties Value Comments
Color Auburn
Users viewing this material also viewed the following: