Material Notes:
Zythane™ 7065D is a polycaprolactone-based TPU specifically formulated for injection molding applications .It exhibits excellent low compression set, abrasion resistance and toughness and has good hydrolytic stability, oil, fuel and solvent resistance. It is supplied uncolored in pellet form. Availability: North AmericaFeatures: Fuel Resistant, Good Toughness, Oil Resistant, Hydrolytically Stable, Solvent Resistant, Good Abrasion Resistance Appearance: ColorlessForms: PelletsProcessing Method: Injection Molding and ExtrusionInformation provided by Alliance Polymers
Physical Properties Metric English Comments
Density 1.18 g/cc
0.0426 lb/in³
ASTM D792
Mechanical Properties Metric English Comments
Hardness, Shore D 65
65
ASTM D2240
Tensile Strength at Break 51.0 MPa
7400 psi
ASTM D412
Tensile Stress 42.0 MPa

@Strain 100 %
6090 psi

@Strain 100 %
ASTM D412
43.0 MPa

@Strain 300 %
6240 psi

@Strain 300 %
ASTM D412
Elongation at Break 350 %
350 %
ASTM D412
Tear Strength 1600 kN/m
9140 pli
Die C; ASTM D412
Taber Abrasion, mg/1000 Cycles 53
53
ASTM D1044
Abrasion 28
28
mm<sup>3</sup>; DIN 53516
Compression Set 38 %

@Temperature 22.8 °C,
Time 79200 sec
38 %

@Temperature 73.0 °F,
Time 22.0 hour
ASTM D3995B
48 %

@Temperature 70.0 °C,
Time 259000 sec
48 %

@Temperature 158 °F,
Time 72.0 hour
ASTM D3995B
Thermal Properties Metric English Comments
Vicat Softening Point 145 °C
293 °F
ASTM D1525
Brittleness Temperature -13.0 °C
8.60 °F
ASTM D746
Flammability, UL94 HB

@Thickness 1.00 mm
HB

@Thickness 0.0394 in
HB

@Thickness 1.50 mm
HB

@Thickness 0.0591 in
HB

@Thickness 3.00 mm
HB

@Thickness 0.118 in
Processing Properties Metric English Comments
Processing Temperature 220 °C
428 °F
Gate Temperature; Extrusion
220 - 230 °C
428 - 446 °F
Injection
Rear Barrel Temperature 205 °C
401 °F
Injection
Middle Barrel Temperature 215 °C
419 °F
Injection
Front Barrel Temperature 225 °C
437 °F
Injection
Nozzle Temperature 220 - 230 °C
428 - 446 °F
Injection
Zone 1 205 °C
401 °F
Extrusion
Zone 2 215 °C
419 °F
Extrusion
Zone 3 225 °C
437 °F
Extrusion
Die Temperature 230 °C
446 °F
Extrusion
Mold Temperature 25.0 - 60.0 °C
77.0 - 140 °F
Injection
Injection Velocity >= 10.0 mm/sec
>= 0.394 in/sec
Injection
Drying Temperature 90.0 °C
194 °F
Injection
90.0 °C
194 °F
Extrusion
Dry Time 4.00 hour
4.00 hour
Injection
4.00 hour
4.00 hour
Extrusion
Back Pressure 0.600 - 1.40 MPa
87.0 - 203 psi
Injection
Clamp Pressure 40.0 - 70.3 MPa
5800 - 10200 psi
Injection
Screw Speed 60 - 200 rpm
60 - 200 rpm
Injection