| Category | Polymer , Thermoplastic , Nylon , Nylon 6 , Nylon 6, 40% Glass Fiber Filled |
| Manufacturer | Gromax |
| Trade Name | |
| Port | Shanghai port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | Gromax CFG35-R113N1 Nylon 6 36% Glass Filled (Dry).pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.40 g/cc | 1.40 g/cc | ISO 1183 |
| Moisture Absorption | 0.860 % | 0.860 % | ISO 62 |
| Maximum Moisture Content | 0.10 | 0.10 | Karl Fischer |
| Linear Mold Shrinkage, Flow | 0.0030 cm/cm @Temperature 80.0 °C |
0.0030 in/in @Temperature 176 °F |
60x60x2 mm; ISO 294-4 |
| Linear Mold Shrinkage, Transverse | 0.0070 cm/cm @Temperature 80.0 °C |
0.0070 in/in @Temperature 176 °F |
60x60x2 mm; ISO 294-4 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Shore D | 88 | 88 | [N/mm<sup>2<sup>]; ISO 7619 |
| Tensile Strength | 182 MPa | 26500 psi | 50 mm/min; ISO 527 |
| Elongation at Break | 3.3 % | 3.3 % | 50 mm/min; ISO 527 |
| Flexural Strength | 260 MPa | 37700 psi | 5 mm/min; ISO 178 |
| Flexural Modulus | 8.83 GPa | 1280 ksi | 5 mm/min; ISO 178 |
| Izod Impact, Notched (ISO) | 17.0 kJ/m² | 8.09 ft-lb/in² | ISO 180-1A |
| Charpy Impact Unnotched | 9.00 J/cm² @Temperature 23.0 °C |
42.8 ft-lb/in² @Temperature 73.4 °F |
ISO 179-1eU |
| Charpy Impact, Notched | 1.77 J/cm² @Temperature 23.0 °C |
8.42 ft-lb/in² @Temperature 73.4 °F |
ISO 179-1A |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| Deflection Temperature at 1.8 MPa (264 psi) | 226 °C | 439 °F | ISO 75-1,-2 |
| Flammability, UL94 | HB @Thickness 1.60 mm |
HB @Thickness 0.0630 in |
| Processing Properties | Metric | English | Comments |
|---|---|---|---|
| Melt Temperature | 266 - 280 °C | 511 - 536 °F | ISO 294 |
| Mold Temperature | 80.0 - 120 °C | 176 - 248 °F | ISO 294 |
| Drying Temperature | 80.0 °C | 176 °F | |