| Category | Polymer , Thermoplastic , Polyester, TP , Polybutylene Terephthalate (PBT) |
| Manufacturer | LG Chemical |
| Trade Name | Lupox® |
| Port | Shanghai port,China |
| Trade Terms | FOB, CFR, CIF |
| Payment Terms | L/C, T/T, Western Union |
| Download PDF | LG Chemical Lupox® GP1000M PBT.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.28 g/cc | 1.28 g/cc | ASTM D792 |
| Maximum Moisture Content | 0.020 | 0.020 | Injection Molding |
| Linear Mold Shrinkage, Flow | 0.012 - 0.020 cm/cm @Thickness 3.20 mm |
0.012 - 0.020 in/in @Thickness 0.126 in |
ASTM D955 |
| Melt Flow | 35 g/10 min @Load 2.16 kg, Temperature 250 °C |
35 g/10 min @Load 4.76 lb, Temperature 482 °F |
ASTM D1238 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength, Yield | 46.1 MPa @Thickness 3.20 mm |
6680 psi @Thickness 0.126 in |
50mm/min; ASTM D638 |
| Elongation at Break | >= 100 % @Thickness 3.20 mm |
>= 100 % @Thickness 0.126 in |
50mm/min; ASTM D638 |
| Flexural Yield Strength | 70.6 MPa @Thickness 3.20 mm |
10200 psi @Thickness 0.126 in |
2.8mm/min; ASTM D790 |
| Flexural Modulus | 1.96 GPa @Thickness 3.20 mm |
284 ksi @Thickness 0.126 in |
2.8mm/min; ASTM D790 |
| Izod Impact, Notched | 0.490 J/cm @Thickness 3.20 mm, Temperature 23.0 °C |
0.918 ft-lb/in @Thickness 0.126 in, Temperature 73.4 °F |
ASTM D256 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| Melting Point | 225 °C | 437 °F | @ Break; ASTM D3418 |
| Deflection Temperature at 0.46 MPa (66 psi) | 154 °C @Thickness 6.40 mm |
309 °F @Thickness 0.252 in |
Unannealed; ASTM D648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 54.0 °C @Thickness 6.40 mm |
129 °F @Thickness 0.252 in |
Unannealed; ASTM D648 |
| UL RTI, Electrical | 140 °C @Thickness >=0.710 mm |
284 °F @Thickness >=0.0280 in |
|
| 140 °C @Thickness >=1.50 mm |
284 °F @Thickness >=0.0591 in |
||
| 140 °C @Thickness >=3.30 mm |
284 °F @Thickness >=0.130 in |
||
| UL RTI, Mechanical with Impact | 130 °C @Thickness >=0.710 mm |
266 °F @Thickness >=0.0280 in |
|
| 130 °C @Thickness >=1.50 mm |
266 °F @Thickness >=0.0591 in |
||
| 130 °C @Thickness >=3.30 mm |
266 °F @Thickness >=0.130 in |
||
| UL RTI, Mechanical without Impact | 140 °C @Thickness >=0.710 mm |
284 °F @Thickness >=0.0280 in |
|
| 140 °C @Thickness >=1.50 mm |
284 °F @Thickness >=0.0591 in |
||
| 140 °C @Thickness >=3.30 mm |
284 °F @Thickness >=0.130 in |
||
| Flammability, UL94 | HB @Thickness >=0.710 mm |
HB @Thickness >=0.0280 in |
|
| HB @Thickness >=1.50 mm |
HB @Thickness >=0.0591 in |
||
| HB @Thickness >=3.30 mm |
HB @Thickness >=0.130 in |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Volume Resistivity | 1.00e+17 ohm-cm | 1.00e+17 ohm-cm | ASTM D257 |
| Dielectric Strength | 23.0 kV/mm @Thickness 1.00 mm |
584 kV/in @Thickness 0.0394 in |
ASTM D149 |
| Arc Resistance | 120 - 180 sec | 120 - 180 sec | ASTM D495 |
| Comparative Tracking Index | 600 V | 600 V | Solution A; IEC 60112 |
| Hot Wire Ignition, HWI | 7.0 - 15 sec @Thickness >=1.50 mm |
7.0 - 15 sec @Thickness >=0.0591 in |
|
| 15 - 30 sec @Thickness >=3.30 mm |
15 - 30 sec @Thickness >=0.130 in |
||
| High Amp Arc Ignition, HAI | >= 120 arcs @Thickness 1.50 mm |
>= 120 arcs @Thickness 0.0591 in |
|
| >= 120 arcs @Thickness 3.30 mm |
>= 120 arcs @Thickness 0.130 in |
| Processing Properties | Metric | English | Comments |
|---|---|---|---|
| Rear Barrel Temperature | 230 - 235 °C | 446 - 455 °F | Injection Molding |
| Middle Barrel Temperature | 235 - 245 °C | 455 - 473 °F | Injection Molding |
| Front Barrel Temperature | 235 - 245 °C | 455 - 473 °F | Injection Molding |
| Nozzle Temperature | 240 - 250 °C | 464 - 482 °F | Injection Molding |
| Melt Temperature | 240 - 250 °C | 464 - 482 °F | Injection Molding |
| Mold Temperature | 40.0 - 80.0 °C | 104 - 176 °F | Injection Molding |
| Drying Temperature | 100 - 120 °C | 212 - 248 °F | Injection Molding |
| Dry Time | 3.00 - 5.00 hour | 3.00 - 5.00 hour | Injection Molding |