Solvay Specialty Polymers Veradel® 3320GF Polyethersulfone (PESU), 20% Glass Fiber

Category Polymer , Thermoplastic , Polyethersulfone (PES) , Polyethersulfone (PES), 20%Glass Fiber Filled
Manufacturer Solvay Specialty Polymers
Trade Name Veradel®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Solvay Specialty Polymers Veradel® 3320GF Polyethersulfone (PESU), 20% Glass Fiber.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Veradel® 3320GF is a 20% glass fiber reinforced grade of polyethersulfone (PESU). Adding glass fiber to polyethersulfone substantially increases the rigidity, tensile strength, creep resistance, dimensional stability and chemical resistance of the material, while maintaining most of its other basic characteristics. The combination of structural properties and cost effectiveness make this resin an attractive alternative to metals in many engineering applications. Veradel® 3320GF is an opaque, grayish material in its natural form and can be readily colored.Features: Acid Resistant; Flame Retardant; Good Adhesion; Good Creep Resistance; Good Dimensional Stability; High Rigidity; High Tensile Strength; Hydrolysis Resistant; Medium Flow; Medium Molecular WeightUses: Metal ReplacementInformation provided by Solvay Specialty Polymers.
Physical Properties Metric English Comments
Density 1.49 g/cc
0.0538 lb/in³
ASTM D792
Filler Content 20 %
20 %
Glass Fiber
Water Absorption 0.50 %

@Time 86400 sec
0.50 %

@Time 24.0 hour
ISO 62
Linear Mold Shrinkage, Flow 0.0030 cm/cm
0.0030 in/in
Mechanical Properties Metric English Comments
Tensile Strength 120 MPa
17400 psi
ASTM D638
Elongation at Break 2.8 %
2.8 %
ASTM D638
Tensile Modulus 7.00 GPa
1020 ksi
ASTM D638
Flexural Strength 170 MPa
24700 psi
ASTM D790
Flexural Modulus 6.50 GPa
943 ksi
ASTM D790
Izod Impact, Notched 0.700 J/cm
1.31 ft-lb/in
ASTM D256
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 25.0 µm/m-°C
13.9 µin/in-°F
Maximum Service Temperature, Air 190 °C
374 °F
Continuous Use
Deflection Temperature at 1.8 MPa (264 psi) 210 °C
410 °F
Annealed; ASTM D648
Flammability, UL94 V-0

@Thickness 0.800 mm
V-0

@Thickness 0.0315 in
Oxygen Index 42 %
42 %
ASTM D2863
Electrical Properties Metric English Comments
Volume Resistivity 1.00e+16 ohm-cm
1.00e+16 ohm-cm
ASTM D257
Surface Resistance 1.00e+14 ohm
1.00e+14 ohm
ASTM D257
Dielectric Strength 20.0 kV/mm
508 kV/in
ASTM D149
Arc Resistance 110 sec
110 sec
ASTM D495
Comparative Tracking Index 150 V
150 V
UL 746
Processing Properties Metric English Comments
Melt Temperature 340 - 380 °C
644 - 716 °F
Mold Temperature 120 - 160 °C
248 - 320 °F
Die Cooling Temperature 300 - 320 °C
572 - 608 °F
Drying Temperature 150 °C

@Time 10800 sec
302 °F

@Time 3.00 hour
Screw Speed 20 - 50 rpm
20 - 50 rpm
Descriptive Properties Value Comments
Availability Africa & Middle East
Asia Pacific
Europe
Latin America
North America
Color Colors Available; Opaque
Form Pellets
Processing Technique Injection Molding
RoHS Compliance RoHS Compliant