Material Notes:
Product description: Grilon BGZ-40 is a normal viscosity, heat stabilized and impact modified PA 6 injection molding type with 40% glass fibers. Grilon BGZ-40 has the following important properties: Good impact strengthHigh stiffnessEasy processingApplication examples are structural components for furniture applications, housings for electro power tools and functional parts for automotive applications.Information provided by EMS Grivory
Physical Properties Metric English Comments
Density 1.43 g/cc
0.0517 lb/in³
ISO 1183
Water Absorption 5.0 %
5.0 %
ISO 62
Moisture Absorption 1.50 %
1.50 %
ISO 62
Linear Mold Shrinkage, Flow 0.0010 cm/cm
0.0010 in/in
ISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0050 cm/cm
0.0050 in/in
ISO 294-4, 2577
Mechanical Properties Metric English Comments
Ball Indentation Hardness 120 MPa
17400 psi
conditioned; ISO 2039-1
220 MPa
31900 psi
dry; ISO 2039-1
Tensile Strength at Break 115 MPa
16700 psi
conditioned; ISO 527-1/-2
170 MPa
24700 psi
dry; ISO 527-1/-2
Elongation at Break 3.5 %
3.5 %
dry; ISO 527-1/-2
8.0 %
8.0 %
conditioned; ISO 527-1/-2
Tensile Modulus 7.50 GPa
1090 ksi
conditioned; ISO 527-1/-2
11.0 GPa
1600 ksi
dry; ISO 527-1/-2
Charpy Impact Unnotched 10.0 J/cm²
47.6 ft-lb/in²
dry; ISO 179/1eU
12.0 J/cm²
57.1 ft-lb/in²
conditioned; ISO 179/1eU
8.50 J/cm²

@Temperature 30.0 °C
40.4 ft-lb/in²

@Temperature 86.0 °F
dry; ISO 179/1eU
10.0 J/cm²

@Temperature 30.0 °C
47.6 ft-lb/in²

@Temperature 86.0 °F
conditioned; ISO 179/1eU
Charpy Impact, Notched 2.50 J/cm²
11.9 ft-lb/in²
dry; ISO 179/1eA
3.50 J/cm²
16.7 ft-lb/in²
conditioned; ISO 179/1eA
1.90 J/cm²

@Temperature 30.0 °C
9.04 ft-lb/in²

@Temperature 86.0 °F
dry; ISO 179/1eU
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 20.0 µm/m-°C
11.1 µin/in-°F
ISO 11359-1/-2
CTE, linear, Transverse to Flow 60.0 µm/m-°C
33.3 µin/in-°F
ISO 11359-1/-2
Melting Point 222 °C
432 °F
10°C/min; ISO 11357-1/-3
Maximum Service Temperature, Air 90.0 - 120 °C
194 - 248 °F
long term; EMS
160 °C
320 °F
short term; EMS
Deflection Temperature at 1.8 MPa (264 psi) 205 °C
401 °F
ISO 75-1/-2
Deflection Temperature at 8.0 MPa 120 °C
248 °F
ISO 75-1/-2
Flammability, UL94 HB
HB
IEC 60695-11-10
Electrical Properties Metric English Comments
Volume Resistivity 1.00e+13 ohm-cm
1.00e+13 ohm-cm
conditioned; IEC 60093
1.00e+14 ohm-cm
1.00e+14 ohm-cm
dry; IEC 60093
Surface Resistance 1.00e+12 ohm
1.00e+12 ohm
IEC 60093
Dielectric Strength 37.0 kV/mm
940 kV/in
conditioned; IEC 60243-1
41.0 kV/mm
1040 kV/in
dry; IEC 60243-1
Comparative Tracking Index 550 V
550 V
conditioned; IEC 60112
Descriptive Properties Value Comments
Form Granules
Processing Injection Molding
Special Characteristics High impact or impact modified