Material Notes:
Polyvinyl chloride is a flame retardant material with an exceptional chemical resistance and also with lower stress cracking. PVC-U shows high mechanical strength, tensile strength and the continuous operating temperature is from -15°C to 60°C. It can also be easily solvent, cemented and welded. Properties include: High mechanical strength, tensile strength and hardnessGood insulation properties for electronicsHigh chemical resistanceSelf-extinguishingLow water absorptionEasy to varnish and glueLow impact strengthLimited weather resistanceApplications include:Pumps and valve bodyGasketsBearing cagesPipe linesHand pump pipesBrush basic bodyParts in the dental medicineSeat stripsPipes for the mounting of kerfsLamp box PVC-C has high rigidity, strength, and hardness at increased temperatures.
Physical Properties Metric English Comments
Specific Gravity 1.55 g/cc
1.55 g/cc
ISO 1183
Water Absorption 0.20 %
0.20 %
ISO 62
Mechanical Properties Metric English Comments
Hardness, Shore D 90
90
DIN 53505
Ball Indentation Hardness 150 MPa
21800 psi
ISO 2039
Tensile Strength at Break 80.0 MPa
11600 psi
ISO 527
Tensile Strength, Yield 57.0 MPa
8270 psi
ISO 527
Elongation at Break 15 %
15 %
ISO 527
Elongation at Yield 3.0 %
3.0 %
ISO 527
Modulus of Elasticity 2.50 GPa
363 ksi
ISO 527
Flexural Strength 90.0 MPa
13100 psi
3.5%; ISO 178
Charpy Impact Unnotched NB
NB
ISO 179
Charpy Impact, Notched 7.00 J/cm²
33.3 ft-lb/in²
ISO 179
Coefficient of Friction 0.60
0.60
DIN 53375
Thermal Properties Metric English Comments
CTE, linear 60.0 µm/m-°C

@Temperature 20.0 °C
33.3 µin/in-°F

@Temperature 68.0 °F
DIN 53752
Thermal Conductivity 0.140 W/m-K
0.972 BTU-in/hr-ft²-°F
DIN 52612
Maximum Service Temperature, Air 85.0 °C
185 °F
Deflection Temperature at 0.46 MPa (66 psi) 102 °C
216 °F
ISO 75
Vicat Softening Point 105 °C
221 °F
VST/B/50; ISO 306
Minimum Service Temperature, Air -15.0 °C
5.00 °F
Flammability, UL94 V-0
V-0
Electrical Properties Metric English Comments
Volume Resistivity >= 1.00e+15 ohm-cm
>= 1.00e+15 ohm-cm
VDE 0303
Surface Resistivity per Square >= 1.00e+13 ohm
>= 1.00e+13 ohm
VDE 0303
Dielectric Constant 3.0

@Frequency 1.00e+6 Hz
3.0

@Frequency 1.00e+6 Hz
DIN 53483
Dielectric Strength 20.0 - 40.0 kV/mm
508 - 1020 kV/in
VDE 0303
Dielectric Loss Index 0.010

@Frequency 1.00e+6 Hz
0.010

@Frequency 1.00e+6 Hz
DIN 53483
Comparative Tracking Index 600 V
600 V
KB; IEC 60112
Descriptive Properties Value Comments
Acid Resistance yes
Aromatic Resistance limited
Bondability yes
Chemical Resistance DIN 8061
CKW Resistance no
Color Light Grey
Hydrocarbonate Resistance yes
Hydroxide Resistance yes
Ketone Resistance limited
Physiological indifference according no
Resistance Against Hot Water limited
UV Stabilization no
Users viewing this material also viewed the following: