Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Nylon 6, Unreinforced". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 0.970 - 4.50 g/cc
0.0350 - 0.163 lb/in³
Average value: 1.13 g/cc Grade Count:526
0.980 - 0.980 g/cc

@Temperature 285 - 285 °C
0.0354 - 0.0354 lb/in³

@Temperature 545 - 545 °F
Average value: 0.980 g/cc Grade Count:1
Apparent Bulk Density 0.425 - 0.800 g/cc
0.0154 - 0.0289 lb/in³
Average value: 0.650 g/cc Grade Count:12
Water Absorption 0.300 - 11.0 %
0.300 - 11.0 %
Average value: 4.91 % Grade Count:285
Moisture Absorption at Equilibrium 0.0400 - 9.50 %
0.0400 - 9.50 %
Average value: 2.79 % Grade Count:221
Water Absorption at Saturation 6.50 - 10.0 %
6.50 - 10.0 %
Average value: 9.00 % Grade Count:49
Oxygen Transmission Rate 40.3 cc/m²/day
2.60 cc/100 in²/day
Average value: 40.3 cc/m²/day Grade Count:10
Nitrogen Transmission 14.0 cc-mm/m²-24hr-atm
35.6 cc-mil/100 in²-24hr-atm
Average value: 14.0 cc-mm/m²-24hr-atm Grade Count:10
Carbon Dioxide Transmission 72.8 cc-mm/m²-24hr-atm
185 cc-mil/100 in²-24hr-atm
Average value: 72.8 cc-mm/m²-24hr-atm Grade Count:10
Viscosity 2.60 - 50.0 cP
2.60 - 50.0 cP
Average value: 8.83 cP Grade Count:17
150000 - 350000 cP

@Temperature 230 - 290 °C
150000 - 350000 cP

@Temperature 446 - 554 °F
Average value: 213000 cP Grade Count:1
150000 - 350000 cP

@Shear Rate 0.100 - 1000 1/s
150000 - 350000 cP

@Shear Rate 0.100 - 1000 1/s
Average value: 213000 cP Grade Count:1
Viscosity Test 118 - 450 cm³/g
118 - 450 cm³/g
Average value: 190 cm³/g Grade Count:44
Maximum Moisture Content 0.100
0.100
Average value: 0.100 Grade Count:22
Linear Mold Shrinkage 0.00130 - 0.0508 cm/cm
0.00130 - 0.0508 in/in
Average value: 0.0137 cm/cm Grade Count:296
Linear Mold Shrinkage, Transverse 0.00110 - 0.0300 cm/cm
0.00110 - 0.0300 in/in
Average value: 0.0132 cm/cm Grade Count:94
Melt Flow 1.00 - 198 g/10 min
1.00 - 198 g/10 min
Average value: 59.2 g/10 min Grade Count:59
Spiral Flow 55.0 - 65.0 cm
21.7 - 25.6 in
Average value: 60.7 cm Grade Count:6
Mechanical Properties Metric English Comments
Hardness, Rockwell M 82.0 - 88.0
82.0 - 88.0
Average value: 85.0 Grade Count:5
Hardness, Rockwell R 78.0 - 120
78.0 - 120
Average value: 113 Grade Count:92
Hardness, Shore D 61.0 - 85.0
61.0 - 85.0
Average value: 69.7 Grade Count:22
Ball Indentation Hardness 50.0 - 190 MPa
7250 - 27600 psi
Average value: 119 MPa Grade Count:32
Tensile Strength, Ultimate 20.0 - 110 MPa
2900 - 16000 psi
Average value: 67.7 MPa Grade Count:184
29.0 - 80.0 MPa

@Temperature -40.0 - 120 °C
4210 - 11600 psi

@Temperature -40.0 - 248 °F
Average value: 45.0 MPa Grade Count:4
10.0 - 100 MPa

@Temperature -20.0 - 100 °C
1450 - 14500 psi

@Temperature -4.00 - 212 °F
Average value: 45.0 MPa Grade Count:2
10.0 - 100 MPa

@Strain 1.00 - 8.00 %
1450 - 14500 psi

@Strain 1.00 - 8.00 %
Average value: 45.0 MPa Grade Count:2
Tensile Strength, Yield 3.45 - 100 MPa
500 - 14500 psi
Average value: 63.2 MPa Grade Count:310
20.0 - 142 MPa

@Temperature -40.0 - 121 °C
2900 - 20600 psi

@Temperature -40.0 - 250 °F
Average value: 74.0 MPa Grade Count:16
Elongation at Break 0.400 - 500 %
0.400 - 500 %
Average value: 76.9 % Grade Count:405
2.50 - 2.50 %

@Temperature -40.0 - -40.0 °C
2.50 - 2.50 %

@Temperature -40.0 - -40.0 °F
Average value: 2.50 % Grade Count:1
Elongation at Yield 3.00 - 140 %
3.00 - 140 %
Average value: 13.9 % Grade Count:178
3.00 - 42.0 %

@Temperature -40.0 - 121 °C
3.00 - 42.0 %

@Temperature -40.0 - 250 °F
Average value: 34.3 % Grade Count:5
Modulus of Elasticity 0.350 - 13.0 GPa
50.8 - 1890 ksi
Average value: 2.29 GPa Grade Count:251
0.360 - 3.75 GPa

@Temperature -40.0 - 120 °C
52.2 - 544 ksi

@Temperature -40.0 - 248 °F
Average value: 1.69 GPa Grade Count:4
Flexural Yield Strength 16.0 - 200 MPa
2320 - 29000 psi
Average value: 82.1 MPa Grade Count:285
8.00 - 183 MPa

@Temperature -40.0 - 250 °C
1160 - 26500 psi

@Temperature -40.0 - 482 °F
Average value: 86.7 MPa Grade Count:16
Flexural Modulus 0.100 - 9.50 GPa
14.5 - 1380 ksi
Average value: 2.15 GPa Grade Count:327
0.260 - 3.90 GPa

@Temperature -40.0 - 121 °C
37.7 - 566 ksi

@Temperature -40.0 - 250 °F
Average value: 1.29 GPa Grade Count:14
Compressive Yield Strength 6.00 - 96.5 MPa
870 - 14000 psi
Average value: 48.0 MPa Grade Count:7
Poissons Ratio 0.350 - 0.450
0.350 - 0.450
Average value: 0.372 Grade Count:5
Izod Impact, Notched 0.370 J/cm - NB
0.693 ft-lb/in - NB
Average value: 1.42 J/cm Grade Count:206
0.210 - 2.10 J/cm

@Temperature -40.0 - -20.0 °C
0.393 - 3.93 ft-lb/in

@Temperature -40.0 - -4.00 °F
Average value: 0.784 J/cm Grade Count:19
0.534 - 2.54973 J/cm

@Temperature -40.0 - -30.0 °C
1.00 - 4.77669 ft-lb/in

@Temperature -40.0 - -22.0 °F
Average value: 0.784 J/cm Grade Count:4
0.534 - 2.54973 J/cm

@Thickness 1.57 - 6.40 mm
1.00 - 4.77669 ft-lb/in

@Thickness 0.0618 - 0.252 in
Average value: 0.784 J/cm Grade Count:4
Izod Impact, Unnotched 0.587 J/cm - NB
1.10 ft-lb/in - NB
Average value: 7.66 J/cm Grade Count:8
Izod Impact, Notched (ISO) 3.50 kJ/m² - NB
1.67 ft-lb/in² - NB
Average value: 30.8 kJ/m² Grade Count:73
3.00 kJ/m² - NB

@Temperature -40.0 - -20.0 °C
1.43 ft-lb/in² - NB

@Temperature -40.0 - -4.00 °F
Average value: 12.4 kJ/m² Grade Count:20
Izod Impact, Unnotched (ISO) 35.0 kJ/m² - NB
16.7 ft-lb/in² - NB
Average value: 61.8 kJ/m² Grade Count:9
200 kJ/m² - NB

@Temperature -30.0 - -30.0 °C
95.2 ft-lb/in² - NB

@Temperature -22.0 - -22.0 °F
Average value: 250 kJ/m² Grade Count:5
Charpy Impact Unnotched 0.800 J/cm² - NB
3.81 ft-lb/in² - NB
Average value: 10.6 J/cm² Grade Count:198
1.60 J/cm² - NB

@Temperature -40.0 - -20.0 °C
7.61 ft-lb/in² - NB

@Temperature -40.0 - -4.00 °F
Average value: 11.0 J/cm² Grade Count:102
Charpy Impact, Notched 0.110 J/cm² - NB
0.524 ft-lb/in² - NB
Average value: 2.47 J/cm² Grade Count:211
0.150 J/cm² - NB

@Temperature -40.0 - -20.0 °C
0.714 ft-lb/in² - NB

@Temperature -40.0 - -4.00 °F
Average value: 0.997 J/cm² Grade Count:99
Gardner Impact 36.2 J
26.7 ft-lb
Average value: 36.2 J Grade Count:5
Dart Drop, Total Energy 67.8 - 285 J
50.0 - 210 ft-lb
Average value: 204 J Grade Count:4
Users viewing this material also viewed the following: