| Category | Polymer , Thermoplastic , Polycarbonate (PC) , Polycarbonate, Molded |
| Manufacturer | |
| Trade Name | |
| Port | Ningbo port,China |
| Trade Terms | FOB, CFR, CIF |
| Payment Terms | L/C, T/T, Western Union |
| Download PDF | Covestro Apec® DP 1-9389 Polycarbonate
(discontinued **).pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 0.960 g/cc | 0.0347 lb/in³ | Melt |
| 1.12 g/cc | 0.0405 lb/in³ | ||
| Water Absorption | 0.40 % | 0.40 % | |
| Moisture Absorption at Equilibrium | 0.20 % | 0.20 % | 23°C/50% R.H. |
| Melt Flow | 4.0 g/10 min @Load 2.16 kg, Temperature 330 °C |
4.0 g/10 min @Load 4.76 lb, Temperature 626 °F |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength, Yield | 65.0 MPa | 9430 psi | |
| Elongation at Break | 50 % | 50 % | Nominal |
| Elongation at Yield | 7.0 % | 7.0 % | |
| Tensile Modulus | 2.30 GPa | 334 ksi | |
| Charpy Impact Unnotched | NB | NB | |
| NB @Temperature -30.0 °C |
NB @Temperature -22.0 °F |
||
| Charpy Impact, Notched | 0.600 J/cm² | 2.86 ft-lb/in² | |
| 0.600 J/cm² @Temperature -30.0 °C |
2.86 ft-lb/in² @Temperature -22.0 °F |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 70.0 µm/m-°C @Temperature 20.0 °C |
38.9 µin/in-°F @Temperature 68.0 °F |
|
| CTE, linear, Transverse to Flow | 70.0 µm/m-°C @Temperature 20.0 °C |
38.9 µin/in-°F @Temperature 68.0 °F |
|
| Specific Heat Capacity | 1.70 J/g-°C | 0.406 BTU/lb-°F | Melt |
| Thermal Conductivity | 0.163 W/m-K | 1.13 BTU-in/hr-ft²-°F | Melt |
| Deflection Temperature at 0.46 MPa (66 psi) | 208 °C | 406 °F | |
| Deflection Temperature at 1.8 MPa (264 psi) | 185 °C | 365 °F | |
| Vicat Softening Point | 218 °C | 424 °F | 50°C/h 50N |
| Flammability, UL94 | HB @Thickness 1.50 mm |
HB @Thickness 0.0591 in |
|
| HB @Thickness 3.00 mm |
HB @Thickness 0.118 in |
||
| Oxygen Index | 24 % | 24 % |
| Optical Properties | Metric | English | Comments |
|---|---|---|---|
| Transmission, Visible | 80 % | 80 % | Manufacturer states transparent but does not quantify |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Volume Resistivity | >= 1.00e+13 ohm-cm | >= 1.00e+13 ohm-cm | |
| Surface Resistance | >= 1.00e+15 ohm | >= 1.00e+15 ohm | |
| Dielectric Constant | 2.9 @Frequency 100 Hz |
2.9 @Frequency 100 Hz |
|
| 2.9 @Frequency 1e+6 Hz |
2.9 @Frequency 1e+6 Hz |
||
| Dielectric Strength | 35.0 kV/mm | 889 kV/in | |
| Dissipation Factor | 0.0020 @Frequency 100 Hz |
0.0020 @Frequency 100 Hz |
|
| 0.0070 @Frequency 1e+6 Hz |
0.0070 @Frequency 1e+6 Hz |
||
| Comparative Tracking Index | 600 V | 600 V |
| Processing Properties | Metric | English | Comments |
|---|---|---|---|
| Melt Temperature | 330 °C | 626 °F | Injection Molding |
| Mold Temperature | 100 °C | 212 °F | Injection Molding |
| Ejection Temperature | 200 °C | 392 °F | |
| Injection Velocity | 200 mm/sec | 7.87 in/sec |
| Descriptive Properties | Value | Comments |
|---|---|---|
| Effective thermal diffusivity | 0.1E-6 m²/s | Melt |