| Category | Polymer , Thermoplastic , Nylon , Nylon 6 , Nylon 6, Glass Fiber Filled, Flame Retardant |
| Manufacturer | Lanxess |
| Trade Name | Durethan® |
| Port | Ningbo port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | Lanxess Durethan® BKV 20 FN20 DUS013 000000 Nylon 6, 20% Glass Fiber.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.35 g/cc | 1.35 g/cc | ISO 1183 |
| Linear Mold Shrinkage, Flow | 0.0010 cm/cm | 0.0010 in/in | Post-shrinkage, 60x60x2; 120°C; 4 hour; ISO 294-4 |
| 0.0060 cm/cm | 0.0060 in/in | 60x60x2; 260°C / MT 80°C; 600 bar; ISO 294-4 | |
| Linear Mold Shrinkage, Transverse | 0.0010 cm/cm | 0.0010 in/in | Post-shrinkage, 60x60x2; 120°C; 4 hour; ISO 294-4 |
| 0.0070 cm/cm | 0.0070 in/in | 60x60x2; 260°C / MT 80°C; 600 bar; ISO 294-4 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 100 MPa | 14500 psi | d.a.m.; ISO 527-1, -2; 5 mm/min |
| Elongation at Break | 3.0 % | 3.0 % | d.a.m.; ISO 527-1, -2; 5 mm/min |
| Tensile Modulus | 6.10 GPa | 885 ksi | d.a.m.; ISO 527-1, -2; 1 mm/min |
| Flexural Strength | 150 MPa @Strain 5.00 % |
21800 psi @Strain 5.00 % |
d.a.m., 2 mm/min; ISO 178-A |
| Flexural Yield Strength | 135 MPa @Strain 3.50 % |
19600 psi @Strain 3.50 % |
d.a.m., 2 mm/min; ISO 178-A |
| Flexural Modulus | 5.70 GPa | 827 ksi | d.a.m., 2 mm/min; ISO 178-A |
| Izod Impact, Notched (ISO) | <= 10.0 kJ/m² | <= 4.76 ft-lb/in² | d.a.m.; ISO 180-1A |
| Izod Impact, Unnotched (ISO) | 30.0 kJ/m² | 14.3 ft-lb/in² | d.a.m.; ISO 180-1U |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| Melting Point | 222 °C | 432 °F | 10°C/min; ISO 11357-1, -3 |
| Deflection Temperature at 1.8 MPa (264 psi) | 185 °C | 365 °F | ISO 75-1, -2 |
| Vicat Softening Point | 205 °C @Load 5.10 kg |
401 °F @Load 11.2 lb |
120°C/hour; ISO 306 |
| Flammability, UL94 | V-2 @Thickness 1.50 mm |
V-2 @Thickness 0.0591 in |
|
| V-2 @Thickness 0.750 mm |
V-2 @Thickness 0.0295 in |
||
| V-2 @Thickness 3.00 mm |
V-2 @Thickness 0.118 in |
||
| Glow Wire Test | 960 °C @Diameter 0.800 mm |
1760 °F @Diameter 0.0315 in |
GWFI; IEC 60695-2-12 |
| 960 °C @Diameter 1.50 mm |
1760 °F @Diameter 0.0591 in |
GWFI; IEC 60695-2-12 | |
| 960 °C @Diameter 3.00 mm |
1760 °F @Diameter 0.118 in |
GWFI; IEC 60695-2-12 |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Comparative Tracking Index | 500 V | 500 V | d.a.m.; Solution A; UL 746A |
| Processing Properties | Metric | English | Comments |
|---|---|---|---|
| Melt Temperature | 250 - 270 °C | 482 - 518 °F | |
| 260 °C | 500 °F | for test specimens; ISO 294 | |
| Mold Temperature | 80.0 °C | 176 °F | for test specimens; ISO 294 |
| 80.0 - 100 °C | 176 - 212 °F | ||
| Drying Temperature | 80.0 °C | 176 °F | |
| Dry Time | 2 - 6 hour | 2 - 6 hour | |
| Moisture Content | 0.030 - 0.070 % | 0.030 - 0.070 % | residual; Karl Fischer Test |
| Descriptive Properties | Value | Comments |
|---|---|---|
| ISO Shortname | ISO 1874-PA 6, GFHR, 12-060, GF20; ISO 1043-PA GF FR(30) |