Overview of materials for Acetal Homopolymer, Unreinforced

Category Polymer , Thermoplastic , Acetal (POM) , Acetal Homopolymer, Unreinforced
Manufacturer
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Acetal Homopolymer, Unreinforced.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Acetal Homopolymer, Unreinforced". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.38 - 1.67 g/cc
0.0499 - 0.0603 lb/in³
Average value: 1.43 g/cc Grade Count:148
1.16 - 1.42 g/cc

@Temperature 200 - 215 °C
0.0419 - 0.0513 lb/in³

@Temperature 392 - 419 °F
Average value: 1.22 g/cc Grade Count:16
Water Absorption 0.0100 - 1.40 %
0.0100 - 1.40 %
Average value: 0.668 % Grade Count:56
Moisture Absorption at Equilibrium 0.170 - 0.500 %
0.170 - 0.500 %
Average value: 0.243 % Grade Count:44
Water Absorption at Saturation 0.200 - 0.900 %
0.200 - 0.900 %
Average value: 0.712 % Grade Count:8
Linear Mold Shrinkage 0.00330 - 0.0400 cm/cm
0.00330 - 0.0400 in/in
Average value: 0.0203 cm/cm Grade Count:116
Linear Mold Shrinkage, Transverse 0.0100 - 0.0300 cm/cm
0.0100 - 0.0300 in/in
Average value: 0.0189 cm/cm Grade Count:61
Melt Flow 1.00 - 70.0 g/10 min
1.00 - 70.0 g/10 min
Average value: 12.4 g/10 min Grade Count:105
Mechanical Properties Metric English Comments
Hardness, Rockwell M 78.0 - 94.0
78.0 - 94.0
Average value: 89.6 Grade Count:45
Hardness, Rockwell R 78.0 - 122
78.0 - 122
Average value: 117 Grade Count:45
Hardness, Shore D 81.0 - 86.0
81.0 - 86.0
Average value: 83.8 Grade Count:4
Ball Indentation Hardness 150 - 192 MPa
21800 - 27800 psi
Average value: 171 MPa Grade Count:5
Tensile Strength, Ultimate 45.0 - 78.0 MPa
6530 - 11300 psi
Average value: 61.9 MPa Grade Count:51
Tensile Strength, Yield 13.0 - 90.0 MPa
1890 - 13100 psi
Average value: 66.5 MPa Grade Count:109
Elongation at Break 2.00 - 80.0 %
2.00 - 80.0 %
Average value: 31.3 % Grade Count:141
Elongation at Yield 1.00 - 40.0 %
1.00 - 40.0 %
Average value: 17.2 % Grade Count:72
Modulus of Elasticity 1.93 - 8.40 GPa
280 - 1220 ksi
Average value: 3.06 GPa Grade Count:116
0.612 - 4.361 GPa

@Temperature -40.0 - 120 °C
88.8 - 632.5 ksi

@Temperature -40.0 - 248 °F
Average value: 2.10 GPa Grade Count:17
Flexural Yield Strength 7.60 - 134 MPa
1100 - 19400 psi
Average value: 84.2 MPa Grade Count:76
Flexural Modulus 1.90 - 6.10 GPa
276 - 885 ksi
Average value: 2.84 GPa Grade Count:113
Compressive Yield Strength 14.0 - 110 MPa
2030 - 16000 psi
Average value: 61.9 MPa Grade Count:7
Poissons Ratio 0.370
0.370
Average value: 0.370 Grade Count:4
Shear Modulus 0.827 - 1.03 GPa
120 - 149 ksi
Average value: 0.922 GPa Grade Count:11
>= 0.121 GPa

@Temperature -50.0 - 150 °C
>= 17.5 ksi

@Temperature -58.0 - 302 °F
Average value: 0.724 GPa Grade Count:11
Shear Strength 55.0 - 62.1 MPa
7980 - 9000 psi
Average value: 59.7 MPa Grade Count:3
Izod Impact, Notched 0.420 - 1.28 J/cm
0.787 - 2.40 ft-lb/in
Average value: 0.679 J/cm Grade Count:53
0.400 - 0.960 J/cm

@Temperature -40.0 - -29.0 °C
0.749 - 1.80 ft-lb/in

@Temperature -40.0 - -20.2 °F
Average value: 0.620 J/cm Grade Count:3
Izod Impact, Unnotched 0.801 J/cm - NB
1.50 ft-lb/in - NB
Average value: 7.52 J/cm Grade Count:12
Izod Impact, Notched (ISO) 3.00 - 14.0 kJ/m²
1.43 - 6.66 ft-lb/in²
Average value: 7.41 kJ/m² Grade Count:39
5.00 - 13.0 kJ/m²

@Temperature -40.0 - -30.0 °C
2.38 - 6.19 ft-lb/in²

@Temperature -40.0 - -22.0 °F
Average value: 8.42 kJ/m² Grade Count:19
Izod Impact, Unnotched (ISO) 20.0 - 280 kJ/m²
9.52 - 133 ft-lb/in²
Average value: 54.6 kJ/m² Grade Count:12
250 - 250 kJ/m²

@Temperature -30.0 - -30.0 °C
119 - 119 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 250 kJ/m² Grade Count:1
Charpy Impact Unnotched 4.00 J/cm² - NB
19.0 ft-lb/in² - NB
Average value: 22.9 J/cm² Grade Count:53
3.50 - 42.5 J/cm²

@Temperature -30.0 - -30.0 °C
16.7 - 202 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 23.5 J/cm² Grade Count:36
Charpy Impact, Notched 0.300 - 1.50 J/cm²
1.43 - 7.14 ft-lb/in²
Average value: 0.892 J/cm² Grade Count:90
0.300 - 1.40 J/cm²

@Temperature -40.0 - -30.0 °C
1.43 - 6.66 ft-lb/in²

@Temperature -40.0 - -22.0 °F
Average value: 0.804 J/cm² Grade Count:49
Gardner Impact 22.6 - 22.6 J
16.7 - 16.7 ft-lb
Average value: 22.6 J Grade Count:6
Tensile Impact Strength 98.1 - 358 kJ/m²
46.7 - 170 ft-lb/in²
Average value: 167 kJ/m² Grade Count:5
Dart Drop, Total Energy 1.00 - 7.00 J
0.738 - 5.16 ft-lb
Average value: 4.50 J Grade Count:8
Coefficient of Friction 0.110 - 0.460
0.110 - 0.460
Average value: 0.262 Grade Count:24
Coefficient of Friction, Static 0.0900 - 0.450
0.0900 - 0.450
Average value: 0.166 Grade Count:16
Tensile Creep Modulus, 1 hour 1500 - 2900 MPa
218000 - 421000 psi
Average value: 2590 MPa Grade Count:11
Tensile Creep Modulus, 1000 hours 800 - 1600 MPa
116000 - 232000 psi
Average value: 1480 MPa Grade Count:11
K (wear) Factor 18.1 - 403 x 10-8 mm³/N-M
9.00 - 200 x 10-10 in³-min/ft-lb-hr
Average value: 60.1 x 10<sup>-8</sup> mm³/N-M Grade Count:12
Limiting Pressure Velocity 0.0513 - 1.08 MPa-m/sec
1460 - 30800 psi-ft/min
Average value: 0.297 MPa-m/sec Grade Count:4
Taber Abrasion, mg/1000 Cycles 10.0 - 13.0
10.0 - 13.0
Average value: 12.0 Grade Count:3
Thermal Properties Metric English Comments
CTE, linear 0.920 - 130 µm/m-°C
0.511 - 72.0 µin/in-°F
Average value: 102 µm/m-°C Grade Count:66
99.0 - 99.0 µm/m-°C

@Temperature 22.8 - 55.0 °C
55.0 - 55.0 µin/in-°F

@Temperature 73.0 - 131 °F
Average value: 99.0 µm/m-°C Grade Count:1
CTE, linear, Transverse to Flow 90.0 - 120 µm/m-°C
50.0 - 66.7 µin/in-°F
Average value: 107 µm/m-°C Grade Count:49
Electrical Properties Metric English Comments
Electrical Resistivity 1.00e+13 - 1.00e+15 ohm-cm
1.00e+13 - 1.00e+15 ohm-cm
Average value: 5.50e+14 ohm-cm Grade Count:27
Surface Resistance 100 - 1.00e+16 ohm
100 - 1.00e+16 ohm
Average value: 1.24e+15 ohm Grade Count:22
Dielectric Constant 3.40 - 4.20
3.40 - 4.20
Average value: 3.79 Grade Count:27
Dielectric Strength 17.7 - 65.0 kV/mm
450 - 1650 kV/in
Average value: 32.0 kV/mm Grade Count:19
Dissipation Factor 0.000500 - 0.0100
0.000500 - 0.0100
Average value: 0.00436 Grade Count:19
Comparative Tracking Index 600 V
600 V
Average value: 600 V Grade Count:19