| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.07 g/cc | 0.0387 lb/in³ | ISO 1183 |
| Water Absorption | 1.65 % | 1.65 % | Equilibrium; ISO 62 |
| 0.45 % @Time 86400 sec |
0.45 % @Time 24.0 hour |
ISO 62 | |
| Moisture Absorption at Equilibrium | 0.35 % | 0.35 % | 23°C/50% RH; ISO 62 |
| Linear Mold Shrinkage, Flow | 0.0040 - 0.0070 cm/cm | 0.0040 - 0.0070 in/in | |
| Melt Flow | 5.885 g/10 min @Load 10.0 kg, Temperature 220 °C |
5.885 g/10 min @Load 22.0 lb, Temperature 428 °F |
ISO 1133 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Ball Indentation Hardness | 65.0 MPa @Load 36.5 kg, Time 30.0 sec |
9430 psi @Load 80.5 lb, Time 0.00833 hour |
ISO 2039-1 |
| Tensile Strength, Yield | 42.0 MPa | 6090 psi | 50 mm/min; ISO 527-1/-2 |
| Elongation at Break | 11 % | 11 % | Nominal, 50 mm/min; ISO 527-1/-2 |
| Elongation at Yield | 3.5 % | 3.5 % | 50 mm/min; ISO 527-1/-2 |
| Tensile Modulus | 2.00 GPa | 290 ksi | ISO 527-1/-2 |
| Flexural Strength | 60.0 MPa | 8700 psi | ISO 178 |
| Poissons Ratio | 0.37 | 0.37 | Calculated |
| Shear Modulus | 0.730 GPa | 106 ksi | ISO 6721-2 |
| Izod Impact, Notched | 6.00 J/cm | 11.2 ft-lb/in | ASTM D256 |
| Charpy Impact Unnotched | 18.0 J/cm² @Temperature -30.0 °C |
85.7 ft-lb/in² @Temperature -22.0 °F |
ISO 179/1eU |
| 25.0 J/cm² @Temperature 23.0 °C |
119 ft-lb/in² @Temperature 73.4 °F |
ISO 179/1eU | |
| Charpy Impact, Notched | 0.900 J/cm² @Temperature -30.0 °C |
4.28 ft-lb/in² @Temperature -22.0 °F |
ISO 179/1eA |
| 4.00 J/cm² @Temperature 23.0 °C |
19.0 ft-lb/in² @Temperature 73.4 °F |
ISO 179/1eA | |
| Tensile Creep Modulus, 1000 hours | 1100 MPa @Strain <=0.500 % |
160000 psi @Strain <=0.500 % |
ISO 899-1 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 80.0 - 110 µm/m-°C @Temperature 23.0 - 80.0 °C |
44.4 - 61.1 µin/in-°F @Temperature 73.4 - 176 °F |
ISO 11359-1/-2 |
| Thermal Conductivity | 0.170 W/m-K | 1.18 BTU-in/hr-ft²-°F | DIN 52612-1 |
| Maximum Service Temperature, Air | 80.0 °C | 176 °F | |
| Deflection Temperature at 0.46 MPa (66 psi) | 100 °C | 212 °F | ISO 75-1/-2 |
| Deflection Temperature at 1.8 MPa (264 psi) | 95.0 °C | 203 °F | ISO 75-1/-2 |
| Vicat Softening Point | 90.0 °C | 194 °F | VST/B/50; ISO 306 |
| 104 °C | 219 °F | VST/A/50; ISO 306 | |
| Flammability, UL94 | HB @Thickness 1.60 mm |
HB @Thickness 0.0630 in |
IEC 60695-11-10 |
| HB @Diameter 4.00 mm |
HB @Diameter 0.157 in |
IEC 60707 |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Volume Resistivity | 1.00e+12 ohm-cm | 1.00e+12 ohm-cm | IEC 60093 |
| Surface Resistance | 1.00e+13 ohm | 1.00e+13 ohm | IEC 60093 |
| Dielectric Constant | 3.3 @Frequency 1.00e+6 Hz |
3.3 @Frequency 1.00e+6 Hz |
IEC 60250 |
| 3.8 @Frequency 100 Hz |
3.8 @Frequency 100 Hz |
IEC 60250 | |
| Dielectric Strength | 35.0 kV/mm | 889 kV/in | K20/P20; IEC 60243-1 |
| Dissipation Factor | 0.0090 @Frequency 100 Hz |
0.0090 @Frequency 100 Hz |
IEC 60250 |
| 0.026 @Frequency 1.00e+6 Hz |
0.026 @Frequency 1.00e+6 Hz |
IEC 60250 | |
| Comparative Tracking Index | 600 V | 600 V | Test Liquid A; IEC 60112 |
| Processing Properties | Metric | English | Comments |
|---|---|---|---|
| Melt Temperature | 240 - 280 °C | 464 - 536 °F | Injection Molding |
| Mold Temperature | 40.0 - 80.0 °C | 104 - 176 °F | Injection Molding |
| Drying Temperature | 80.0 °C | 176 °F | Pre-drying |
| Dry Time | 2 - 4 hour | 2 - 4 hour | Pre-drying |
| Descriptive Properties | Value | Comments |
|---|---|---|
| Color | White 35962 | |
| Commercial Status | Europe | |
| Primary Processing Technique | Injection Molding |