Overview of materials for Epoxy, High Temperature

Category Polymer , Thermoset , Epoxy , Epoxy, High Temperature
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Epoxy, High Temperature.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Epoxy, Encapsulating, Mineral Filled". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 0.990 - 2.26 g/cc
0.0358 - 0.0816 lb/in³
Average value: 1.28 g/cc Grade Count:31
Water Absorption 0.200 - 0.200 %

@Temperature 50.0 - 50.0 °C
0.200 - 0.200 %

@Temperature 122 - 122 °F
Average value: 0.200 % Grade Count:1
0.200 - 0.200 %

@Time 173000 - 173000 sec
0.200 - 0.200 %

@Time 48.0 - 48.0 hour
Average value: 0.200 % Grade Count:1
Particle Size 20.0 - 45.0 µm
20.0 - 45.0 µm
Average value: 25.0 µm Grade Count:9
Viscosity 30.0 - 1.00e+6 cP
30.0 - 1.00e+6 cP
Average value: 45700 cP Grade Count:45
150 - 1800 cP

@Temperature 52.0 - 82.2 °C
150 - 1800 cP

@Temperature 126 - 180 °F
Average value: 767 cP Grade Count:3
Linear Mold Shrinkage 0.00100 - 0.00350 cm/cm
0.00100 - 0.00350 in/in
Average value: 0.00275 cm/cm Grade Count:5
Mechanical Properties Metric English Comments
Hardness, Shore D 40.0 - 96.0
40.0 - 96.0
Average value: 81.2 Grade Count:34
20.0 - 27.0

@Temperature 100 - 177 °C
20.0 - 27.0

@Temperature 212 - 350 °F
Average value: 23.0 Grade Count:2
Tensile Strength, Ultimate 13.8 - 85.0 MPa
2000 - 12300 psi
Average value: 62.3 MPa Grade Count:11
>= 13.7895 MPa

@Temperature 60.0 - 60.0 °C
>= 2000.00 psi

@Temperature 140 - 140 °F
Average value: 13.8 MPa Grade Count:1
Elongation at Break 1.00 - 50.0 %
1.00 - 50.0 %
Average value: 8.25 % Grade Count:8
>= 30.0 %

@Temperature 60.0 - 60.0 °C
>= 30.0 %

@Temperature 140 - 140 °F
Average value: 30.0 % Grade Count:1
Modulus of Elasticity 1.68 - 5.40 GPa
244 - 783 ksi
Average value: 3.00 GPa Grade Count:22
0.827371 - 0.827371 GPa

@Temperature 60.0 - 60.0 °C
120.002 - 120.002 ksi

@Temperature 140 - 140 °F
Average value: 0.827 GPa Grade Count:1
Flexural Yield Strength 79.3 - 160 MPa
11500 - 23200 psi
Average value: 104 MPa Grade Count:9
Compressive Yield Strength 55.2 - 256 MPa
8000 - 37100 psi
Average value: 169 MPa Grade Count:8
Shear Strength 4.83 - 46.9 MPa
700 - 6800 psi
Average value: 20.1 MPa Grade Count:23
Adhesive Bond Strength 15.9 - 27.6 MPa
2300 - 4000 psi
Average value: 20.2 MPa Grade Count:4
6.20528 - 13.7895 MPa

@Temperature 100 - 175 °C
900.002 - 2000.00 psi

@Temperature 212 - 347 °F
Average value: 9.42 MPa Grade Count:1
Izod Impact, Notched 0.155 - 0.481 J/cm
0.290 - 0.900 ft-lb/in
Average value: 0.286 J/cm Grade Count:4
Thermal Properties Metric English Comments
CTE, linear 16.2 - 231 µm/m-°C
9.00 - 128 µin/in-°F
Average value: 97.0 µm/m-°C Grade Count:32
>= 75.0 µm/m-°C

@Temperature 60.0 - 60.0 °C
>= 41.7 µin/in-°F

@Temperature 140 - 140 °F
Average value: 75.0 µm/m-°C Grade Count:1
Thermal Conductivity 0.167 - 1.44 W/m-K
1.16 - 10.0 BTU-in/hr-ft²-°F
Average value: 0.838 W/m-K Grade Count:12
Maximum Service Temperature, Air 149 - 350 °C
300 - 662 °F
Average value: 258 °C Grade Count:55
Minimum Service Temperature, Air -269 - -20.0 °C
-452 - -4.00 °F
Average value: -58.3 °C Grade Count:47
Glass Transition Temp, Tg 30.0 - 220 °C
86.0 - 428 °F
Average value: 108 °C Grade Count:22
Decomposition Temperature 341 - 487 °C
646 - 909 °F
Average value: 405 °C Grade Count:17
Optical Properties Metric English Comments
Refractive Index 1.52 - 1.62
1.52 - 1.62
Average value: 1.57 Grade Count:9
Transmission, Visible 0.100 - 99.0 %
0.100 - 99.0 %
Average value: 77.4 % Grade Count:11
Electrical Properties Metric English Comments
Electrical Resistivity 400 - 1.00e+16 ohm-cm
400 - 1.00e+16 ohm-cm
Average value: 1.31e+15 ohm-cm Grade Count:29
Dielectric Constant 2.58 - 5.20
2.58 - 5.20
Average value: 3.68 Grade Count:29
Dielectric Strength 14.7 - 18.9 kV/mm
373 - 480 kV/in
Average value: 16.9 kV/mm Grade Count:9
Dissipation Factor 0.000700 - 0.0140
0.000700 - 0.0140
Average value: 0.00635 Grade Count:22
Processing Properties Metric English Comments
Processing Temperature 10.0 - 177 °C
50.0 - 350 °F
Average value: 73.0 °C Grade Count:3
Cure Time 30.0 - 4320 min
0.500 - 72.0 hour
Average value: 854 min Grade Count:23
1.00 - 480 min

@Temperature 71.1 - 204 °C
0.0167 - 8.00 hour

@Temperature 160 - 400 °F
Average value: 71.3 min Grade Count:32
Pot Life 8.00 - 7200 min
8.00 - 7200 min
Average value: 670 min Grade Count:33
120 - 120 min

@Temperature 80.0 - 80.0 °C
120 - 120 min

@Temperature 176 - 176 °F
Average value: 120 min Grade Count:1