Material Notes:
Transparent, enhanced flow Polyetherimide (Tg 217C). ECO Conforming. For medical devices and pharmaceutical applications. Healthcare management of change, biocompatible (ISO 10993 or USP Class VI), food contact compliant. EtO and steam sterilizable.
Physical Properties Metric English Comments
Specific Gravity 1.27 g/cc
1.27 g/cc
ASTM D792
Density 1.27 g/cc
0.0459 lb/in³
ISO 1183
Moisture Absorption 0.700 %
0.700 %
23°C / 50% RH; ISO 62
Water Absorption at Saturation 1.25 %
1.25 %
ISO 62
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm

@Thickness 3.20 mm
0.0050 - 0.0070 in/in

@Thickness 0.126 in
SABIC Method
Melt Flow 17.8 g/10 min

@Load 6.60 kg,
Temperature 337 °C
17.8 g/10 min

@Load 14.6 lb,
Temperature 639 °F
ASTM D1238
Melt Index of Compound 25 g/10 min

@Load 5.00 kg,
Temperature 220 °C
25 g/10 min

@Load 11.0 lb,
Temperature 428 °F
MVR [cm^3/10 min]; ISO 1133
Mechanical Properties Metric English Comments
Tensile Strength at Break 85.0 MPa
12300 psi
5 mm/min; ISO 527
105 MPa
15200 psi
Type I, 5 mm/min; ASTM D638
Tensile Strength, Yield 105 MPa
15200 psi
5 mm/min; ISO 527
110 MPa
16000 psi
Type I, 5 mm/min; ASTM D638
Elongation at Break 60 %
60 %
Type I, 5 mm/min; ASTM D638
60 %
60 %
5 mm/min; ISO 527
Elongation at Yield 6.0 %
6.0 %
5 mm/min; ISO 527
7.0 %
7.0 %
Type I, 5 mm/min; ASTM D638
Tensile Modulus 3.20 GPa
464 ksi
1 mm/min; ISO 527
3.58 GPa
519 ksi
5 mm/min; ASTM D638
Flexural Yield Strength 160 MPa
23200 psi
2 mm/min; ISO 178
165 MPa
23900 psi
2.6 mm/min, 100 mm span; ASTM D790
174 MPa
25200 psi
1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 3.30 GPa
479 ksi
2 mm/min; ISO 178
3.42 GPa
496 ksi
1.3 mm/min, 50 mm span; ASTM D790
3.51 GPa
509 ksi
2.6 mm/min, 100 mm span; ASTM D790
Izod Impact, Notched 0.320 J/cm
0.599 ft-lb/in
ASTM D256
0.350 J/cm

@Temperature -30.0 °C
0.656 ft-lb/in

@Temperature -22.0 °F
ASTM D256
Izod Impact, Unnotched 13.35 J/cm
25.01 ft-lb/in
ASTM D4812
Izod Impact, Notched (ISO) 5.00 kJ/m²
2.38 ft-lb/in²
80*10*4; ISO 180/1A
5.00 kJ/m²

@Temperature -30.0 °C
2.38 ft-lb/in²

@Temperature -22.0 °F
80*10*4; ISO 180/1A
Charpy Impact, Notched 0.300 J/cm²
1.43 ft-lb/in²
Edgew 80*10*4 sp=62mm; ISO 179/1eA
Gardner Impact 33.0 J
24.3 ft-lb
ASTM D3029
Dart Drop, Total Energy 33.0 J

@Temperature 23.0 °C
24.3 ft-lb

@Temperature 73.4 °F
ASTM D3763
Taber Abrasion, mg/1000 Cycles 10
10
CS-17, 1 kg; ASTM D1044
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 50.0 µm/m-°C

@Temperature -40.0 - 40.0 °C
27.8 µin/in-°F

@Temperature -40.0 - 104 °F
ISO 11359-2
55.8 µm/m-°C

@Temperature -20.0 - 150 °C
31.0 µin/in-°F

@Temperature -4.00 - 302 °F
ASTM E 831
CTE, linear, Transverse to Flow 50.0 µm/m-°C

@Temperature -40.0 - 40.0 °C
27.8 µin/in-°F

@Temperature -40.0 - 104 °F
ASTM E 831
50.0 µm/m-°C

@Temperature -40.0 - 40.0 °C
27.8 µin/in-°F

@Temperature -40.0 - 104 °F
ISO 11359-2
Deflection Temperature at 1.8 MPa (264 psi) 193 °C
379 °F
Flatw 80*10*4 sp=64mm; ISO 75/Af
198 °C

@Thickness 6.40 mm
388 °F

@Thickness 0.252 in
unannealed; ASTM D648
Vicat Softening Point 211 °C
412 °F
Rate B/50; ISO 306
212 °C
414 °F
Rate B/120; ISO 306
218 °C
424 °F
Rate B/50; ASTM D1525
Glass Transition Temp, Tg 217 °C
423 °F
Flammability, UL94 V-2

@Thickness 0.710 mm
V-2

@Thickness 0.0280 in
UL 94
V-0

@Thickness 0.710 mm
V-0

@Thickness 0.0280 in
UL 94
5VA

@Thickness 2.99 mm
5VA

@Thickness 0.118 in
UL 94
Oxygen Index 44 %
44 %
ASTM D2863
Optical Properties Metric English Comments
Transmission, Visible 90 %
90 %
transparent; thickness not quantified
Electrical Properties Metric English Comments
Volume Resistivity 1.00e+17 ohm-cm
1.00e+17 ohm-cm
ASTM D257
Dielectric Constant 3.15

@Frequency 1000 Hz
3.15

@Frequency 1000 Hz
ASTM D150
Dielectric Strength 27.9 kV/mm

@Thickness 1.60 mm
709 kV/in

@Thickness 0.0630 in
in oil; ASTM D149
32.6 kV/mm

@Thickness 1.60 mm
828 kV/in

@Thickness 0.0630 in
in air; ASTM D149
Dissipation Factor 0.0013

@Frequency 1000 Hz
0.0013

@Frequency 1000 Hz
ASTM D150
0.0025

@Frequency 2.45e+9 Hz
0.0025

@Frequency 2.45e+9 Hz
ASTM D150
Arc Resistance 120 - 180 sec
120 - 180 sec
Tungsten; ASTM D495
Comparative Tracking Index 100 - 175 V
100 - 175 V
UL 746A
Hot Wire Ignition, HWI 60 - 120 sec
60 - 120 sec
UL 746A
High Amp Arc Ignition, HAI 15 - 30 arcs
15 - 30 arcs
UL 746A
High Voltage Arc-Tracking Rate, HVTR 25.4 - 80.0 mm/min
1.00 - 3.15 in/min
UL 746A