Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Acrylic, Impact Modified, Molded". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.04 - 1.19 g/cc
0.0376 - 0.0430 lb/in³
Average value: 1.15 g/cc Grade Count:125
Water Absorption 0.100 - 2.00 %
0.100 - 2.00 %
Average value: 0.366 % Grade Count:61
Moisture Absorption at Equilibrium 0.300 - 0.400 %
0.300 - 0.400 %
Average value: 0.360 % Grade Count:7
Water Absorption at Saturation 0.300 %
0.300 %
Average value: 0.300 % Grade Count:6
Viscosity 975000 - 975000 cP

@Temperature 240 - 240 °C
975000 - 975000 cP

@Temperature 464 - 464 °F
Average value: 975000 cP Grade Count:1
975000 - 975000 cP

@Shear Rate 100 - 100 1/s
975000 - 975000 cP

@Shear Rate 100 - 100 1/s
Average value: 975000 cP Grade Count:1
Linear Mold Shrinkage 0.00200 - 0.00800 cm/cm
0.00200 - 0.00800 in/in
Average value: 0.00504 cm/cm Grade Count:104
Melt Flow 0.700 - 16.0 g/10 min
0.700 - 16.0 g/10 min
Average value: 4.18 g/10 min Grade Count:124
Mechanical Properties Metric English Comments
Hardness, Rockwell M 20.0 - 95.0
20.0 - 95.0
Average value: 56.4 Grade Count:57
Hardness, Rockwell R 61.0 - 117
61.0 - 117
Average value: 78.6 Grade Count:8
Tensile Strength, Ultimate 32.0 - 82.0 MPa
4640 - 11900 psi
Average value: 50.0 MPa Grade Count:107
Tensile Strength, Yield 28.0 - 60.0 MPa
4060 - 8700 psi
Average value: 42.2 MPa Grade Count:17
Elongation at Break 1.90 - 90.0 %
1.90 - 90.0 %
Average value: 30.3 % Grade Count:121
Elongation at Yield 1.90 - 40.0 %
1.90 - 40.0 %
Average value: 5.76 % Grade Count:38
Modulus of Elasticity 1.38 - 3.52 GPa
200 - 510 ksi
Average value: 2.13 GPa Grade Count:92
Flexural Yield Strength 41.2 - 105 MPa
5970 - 15200 psi
Average value: 69.8 MPa Grade Count:110
Flexural Modulus 1.36 - 3.38 GPa
198 - 490 ksi
Average value: 2.11 GPa Grade Count:71
Izod Impact, Notched 0.200 - 2.45 J/cm
0.375 - 4.59 ft-lb/in
Average value: 0.585 J/cm Grade Count:94
0.240255 - 0.37373 J/cm

@Temperature 0.000 - 0.000 °C
0.450096 - 0.70015 ft-lb/in

@Temperature 32.0 - 32.0 °F
Average value: 0.330 J/cm Grade Count:6
0.260 - 0.590 J/cm

@Temperature 0.000 - 0.000 °C
0.487 - 1.11 ft-lb/in

@Temperature 32.0 - 32.0 °F
Average value: 0.330 J/cm Grade Count:2
0.260 - 0.590 J/cm

@Thickness 6.35 - 6.35 mm
0.487 - 1.11 ft-lb/in

@Thickness 0.250 - 0.250 in
Average value: 0.330 J/cm Grade Count:2
0.210 - 0.64068 J/cm

@Diameter 6.35 - 6.35 mm
0.393 - 1.2003 ft-lb/in

@Diameter 0.250 - 0.250 in
Average value: 0.330 J/cm Grade Count:10
0.210 - 0.64068 J/cm

@Temperature 0.000 - 0.000 °C
0.393 - 1.2003 ft-lb/in

@Temperature 32.0 - 32.0 °F
Average value: 0.330 J/cm Grade Count:10
Izod Impact, Unnotched 1.60 J/cm - NB
3.00 ft-lb/in - NB
Average value: 3.92 J/cm Grade Count:7
Izod Impact, Notched (ISO) 2.10 - 8.00 kJ/m²
0.999 - 3.81 ft-lb/in²
Average value: 4.43 kJ/m² Grade Count:19
Izod Impact, Unnotched (ISO) 1.50 - 3.40 kJ/m²
0.714 - 1.62 ft-lb/in²
Average value: 2.14 kJ/m² Grade Count:5
Charpy Impact Unnotched 2.10 - 8.00 J/cm²
9.99 - 38.1 ft-lb/in²
Average value: 5.82 J/cm² Grade Count:18
Charpy Impact, Notched 0.210 - 5.40 J/cm²
0.999 - 25.7 ft-lb/in²
Average value: 1.36 J/cm² Grade Count:26
Gardner Impact 1.58 - 11.0 J
1.17 - 8.11 ft-lb
Average value: 4.61 J Grade Count:47
Thermal Properties Metric English Comments
CTE, linear 60.0 - 123 µm/m-°C
33.3 - 68.3 µin/in-°F
Average value: 90.1 µm/m-°C Grade Count:88
72.0 - 93.6 µm/m-°C

@Temperature 0.000 - 156 °C
40.0 - 52.0 µin/in-°F

@Temperature 32.0 - 312 °F
Average value: 78.6 µm/m-°C Grade Count:6
Specific Heat Capacity 1.90 - 2.30 J/g-°C

@Temperature 100 - 175 °C
0.454 - 0.550 BTU/lb-°F

@Temperature 212 - 347 °F
Average value: 2.10 J/g-°C Grade Count:1
Thermal Conductivity 0.202 - 0.220 W/m-K
1.40 - 1.53 BTU-in/hr-ft²-°F
Average value: 0.210 W/m-K Grade Count:5
Maximum Service Temperature, Air 50.0 - 90.0 °C
122 - 194 °F
Average value: 72.9 °C Grade Count:14
Deflection Temperature at 0.46 MPa (66 psi) 78.0 - 98.0 °C
172 - 208 °F
Average value: 87.8 °C Grade Count:12
Deflection Temperature at 1.8 MPa (264 psi) 73.0 - 111 °C
163 - 232 °F
Average value: 84.4 °C Grade Count:114
Vicat Softening Point 82.0 - 115 °C
180 - 239 °F
Average value: 102 °C Grade Count:122
Annealing Point 60.0 - 70.0 °C
140 - 158 °F
Average value: 65.0 °C Grade Count:8
Heat Distortion Temperature 80.0 - 97.0 °C
176 - 207 °F
Average value: 90.3 °C Grade Count:8
Flammability, UL94 HB
HB
Grade Count:64
Oxygen Index 18.0 - 19.0 %
18.0 - 19.0 %
Average value: 18.2 % Grade Count:6
Glow Wire Test 650 °C
1200 °F
Average value: 650 °C Grade Count:19
Optical Properties Metric English Comments
Refractive Index 1.49 - 1.57
1.49 - 1.57
Average value: 1.50 Grade Count:51
Haze 0.500 - 96.0 %
0.500 - 96.0 %
Average value: 4.05 % Grade Count:92
Yellow Index -1.50 - 5.50 %
-1.50 - 5.50 %
Average value: 0.879 % Grade Count:19
Transmission, Visible 0.000 - 92.0 %
0.000 - 92.0 %
Average value: 86.3 % Grade Count:116
Electrical Properties Metric English Comments
Electrical Resistivity 1.00e+14 - 1.00e+15 ohm-cm
1.00e+14 - 1.00e+15 ohm-cm
Average value: 7.00e+14 ohm-cm Grade Count:15
Surface Resistance 1.00e+14 ohm
1.00e+14 ohm
Average value: 1.00e+14 ohm Grade Count:7
Dielectric Constant 2.90 - 3.90
2.90 - 3.90
Average value: 3.30 Grade Count:15
Dielectric Strength 15.0 - 60.0 kV/mm
381 - 1520 kV/in
Average value: 30.0 kV/mm Grade Count:15
Dissipation Factor 0.0300 - 0.0500
0.0300 - 0.0500
Average value: 0.0386 Grade Count:15
Comparative Tracking Index 600 V
600 V
Average value: 600 V Grade Count:7
Processing Properties Metric English Comments
Processing Temperature 210 - 250 °C
410 - 482 °F
Average value: 230 °C Grade Count:8
Melt Temperature 179 - 260 °C
354 - 500 °F
Average value: 229 °C Grade Count:41
Mold Temperature 27.0 - 107 °C
80.6 - 225 °F
Average value: 61.1 °C Grade Count:39
Drying Temperature 60.0 - 105 °C
140 - 221 °F
Average value: 80.0 °C Grade Count:33