Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Nylon 612, Glass Fiber Filler". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.12 - 1.70 g/cc
0.0405 - 0.0614 lb/in³
Average value: 1.35 g/cc Grade Count:146
1.12 - 1.12 g/cc

@Temperature >=250 °C
0.0405 - 0.0405 lb/in³

@Temperature >=482 °F
Average value: 1.12 g/cc Grade Count:1
Filler Content 5.00 - 60.0 %
5.00 - 60.0 %
Average value: 26.8 % Grade Count:95
Water Absorption 0.0170 - 2.00 %
0.0170 - 2.00 %
Average value: 0.402 % Grade Count:94
Moisture Absorption at Equilibrium 0.100 - 1.00 %
0.100 - 1.00 %
Average value: 0.711 % Grade Count:19
Water Absorption at Saturation 0.300 - 2.60 %
0.300 - 2.60 %
Average value: 1.91 % Grade Count:9
Additive Loading 13.0 - 30.0 %
13.0 - 30.0 %
Average value: 22.6 % Grade Count:5
Viscosity Test 83.0 - 145 cm³/g
83.0 - 145 cm³/g
Average value: 109 cm³/g Grade Count:3
Linear Mold Shrinkage 0.00100 - 0.0300 cm/cm
0.00100 - 0.0300 in/in
Average value: 0.00469 cm/cm Grade Count:144
Linear Mold Shrinkage, Transverse 0.00700 - 0.0170 cm/cm
0.00700 - 0.0170 in/in
Average value: 0.0106 cm/cm Grade Count:22
Mechanical Properties Metric English Comments
Hardness, Rockwell R 114 - 122
114 - 122
Average value: 119 Grade Count:42
Ball Indentation Hardness 145 - 220 MPa
21000 - 31900 psi
Average value: 180 MPa Grade Count:6
Tensile Strength, Ultimate 44.8 - 200 MPa
6500 - 29000 psi
Average value: 131 MPa Grade Count:141
60.0 - 140 MPa

@Temperature 60.0 - 150 °C
8700 - 20300 psi

@Temperature 140 - 302 °F
Average value: 95.6 MPa Grade Count:2
Tensile Strength, Yield 34.0 - 190 MPa
4930 - 27600 psi
Average value: 122 MPa Grade Count:16
Elongation at Break 1.00 - 23.0 %
1.00 - 23.0 %
Average value: 3.80 % Grade Count:141
4.30 - 6.80 %

@Temperature 60.0 - 150 °C
4.30 - 6.80 %

@Temperature 140 - 302 °F
Average value: 5.49 % Grade Count:2
Elongation at Yield 3.00 - 12.0 %
3.00 - 12.0 %
Average value: 5.47 % Grade Count:8
Modulus of Elasticity 2.65 - 17.9 GPa
384 - 2600 ksi
Average value: 8.32 GPa Grade Count:124
1.919 - 15.66 GPa

@Temperature -50.0 - 200 °C
278.3 - 2271 ksi

@Temperature -58.0 - 392 °F
Average value: 6.61 GPa Grade Count:5
Flexural Yield Strength 72.4 - 303 MPa
10500 - 44000 psi
Average value: 193 MPa Grade Count:120
Flexural Modulus 2.76 - 17.9 GPa
400 - 2600 ksi
Average value: 7.33 GPa Grade Count:131
Compressive Yield Strength 89.6 - 179 MPa
13000 - 26000 psi
Average value: 132 MPa Grade Count:27
Shear Modulus 1.65 - 4.22 GPa
239 - 611 ksi
Average value: 2.51 GPa Grade Count:3
>= 0.284 GPa

@Temperature -50.0 - 200 °C
>= 41.2 ksi

@Temperature -58.0 - 392 °F
Average value: 1.48 GPa Grade Count:3
Izod Impact, Notched 0.214 - 1.87 J/cm
0.401 - 3.50 ft-lb/in
Average value: 0.968 J/cm Grade Count:124
Izod Impact, Unnotched 1.33 - 13.3 J/cm
2.50 - 25.0 ft-lb/in
Average value: 7.27 J/cm Grade Count:97
Izod Impact, Notched (ISO) 3.70 - 17.0 kJ/m²
1.76 - 8.09 ft-lb/in²
Average value: 11.3 kJ/m² Grade Count:11
10.0 - 15.0 kJ/m²

@Temperature -40.0 - -30.0 °C
4.76 - 7.14 ft-lb/in²

@Temperature -40.0 - -22.0 °F
Average value: 11.1 kJ/m² Grade Count:7
Izod Impact, Unnotched (ISO) 16.0 - 78.3 kJ/m²
7.61 - 37.3 ft-lb/in²
Average value: 52.6 kJ/m² Grade Count:7
45.0 - 60.0 kJ/m²

@Temperature -30.0 - -30.0 °C
21.4 - 28.6 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 52.5 kJ/m² Grade Count:3
Charpy Impact Unnotched 4.60 - 10.4 J/cm²
21.9 - 49.5 ft-lb/in²
Average value: 8.57 J/cm² Grade Count:21
2.00 - 11.0 J/cm²

@Temperature -30.0 - 30.0 °C
9.52 - 52.4 ft-lb/in²

@Temperature -22.0 - 86.0 °F
Average value: 7.73 J/cm² Grade Count:19
Charpy Impact, Notched 0.400 - 2.00 J/cm²
1.90 - 9.52 ft-lb/in²
Average value: 1.42 J/cm² Grade Count:24
0.300 - 1.70 J/cm²

@Temperature -40.0 - 30.0 °C
1.43 - 8.09 ft-lb/in²

@Temperature -40.0 - 86.0 °F
Average value: 1.07 J/cm² Grade Count:22
Thermal Properties Metric English Comments
CTE, linear 10.0 - 500 µm/m-°C
5.56 - 278 µin/in-°F
Average value: 70.1 µm/m-°C Grade Count:46
14.0 - 500 µm/m-°C

@Temperature 55.0 - 160 °C
7.78 - 278 µin/in-°F

@Temperature 131 - 320 °F
Average value: 154 µm/m-°C Grade Count:6
CTE, linear, Transverse to Flow 46.8 - 113 µm/m-°C
26.0 - 62.8 µin/in-°F
Average value: 86.1 µm/m-°C Grade Count:20
139 - 158 µm/m-°C

@Temperature 55.0 - 160 °C
77.2 - 87.8 µin/in-°F

@Temperature 131 - 320 °F
Average value: 155 µm/m-°C Grade Count:5
Specific Heat Capacity 2.13 J/g-°C
0.509 BTU/lb-°F
Average value: 2.13 J/g-°C Grade Count:3
Thermal Conductivity 0.259 - 0.576 W/m-K
1.80 - 4.00 BTU-in/hr-ft²-°F
Average value: 0.398 W/m-K Grade Count:26
Melting Point 212 - 224 °C
414 - 435 °F
Average value: 216 °C Grade Count:29
Maximum Service Temperature, Air 90.0 - 180 °C
194 - 356 °F
Average value: 139 °C Grade Count:8
Deflection Temperature at 0.46 MPa (66 psi) 169 - 225 °C
336 - 437 °F
Average value: 212 °C Grade Count:87
Deflection Temperature at 1.8 MPa (264 psi) 60.0 - 218 °C
140 - 425 °F
Average value: 199 °C Grade Count:130
Electrical Properties Metric English Comments
Electrical Resistivity 10.0 - 1.00e+16 ohm-cm
10.0 - 1.00e+16 ohm-cm
Average value: 2.73e+14 ohm-cm Grade Count:75
Surface Resistance 100 - 1.00e+15 ohm
100 - 1.00e+15 ohm
Average value: 1.11e+14 ohm Grade Count:9
Dielectric Constant 3.10 - 4.40
3.10 - 4.40
Average value: 3.81 Grade Count:29
Dielectric Strength 18.7 - 38.0 kV/mm
475 - 965 kV/in
Average value: 25.5 kV/mm Grade Count:33
Dissipation Factor 0.0110 - 0.160
0.0110 - 0.160
Average value: 0.0269 Grade Count:28
Arc Resistance 110 - 120 sec
110 - 120 sec
Average value: 117 sec Grade Count:12
Comparative Tracking Index 550 - 600 V
550 - 600 V
Average value: 596 V Grade Count:14