| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.15 g/cc | 1.15 g/cc | ASTM D792 |
| Density | 1.15 g/cc | 0.0415 lb/in³ | ISO 1183 |
| Moisture Absorption | 0.200 % | 0.200 % | 23°C / 50% RH; ISO 62 |
| Water Absorption at Saturation | 0.60 % | 0.60 % | ISO 62 |
| Linear Mold Shrinkage, Flow | 0.0050 - 0.0070 cm/cm | 0.0050 - 0.0070 in/in | on Tensile Bar; SABIC Method |
| 0.0050 - 0.0070 cm/cm @Thickness 3.20 mm |
0.0050 - 0.0070 in/in @Thickness 0.126 in |
SABIC Method | |
| Melt Flow | 24 g/10 min @Load 5.00 kg, Temperature 260 °C |
24 g/10 min @Load 11.0 lb, Temperature 500 °F |
ASTM D1238 |
| Melt Index of Compound | 8.0 g/10 min @Load 2.16 kg, Temperature 260 °C |
8.0 g/10 min @Load 4.76 lb, Temperature 500 °F |
MVR [cm^3/10 min]; ISO 1133 |
| 22 g/10 min @Load 5.00 kg, Temperature 260 °C |
22 g/10 min @Load 11.0 lb, Temperature 500 °F |
MVR [cm^3/10 min]; ISO 1133 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Rockwell R | 115 | 115 | ISO 2039-2 |
| Hardness, H358/30 | 96.0 MPa | 13900 psi | ISO 2039-1 |
| Tensile Strength at Break | 45.0 MPa | 6530 psi | 5 mm/min; ISO 527 |
| 45.0 MPa | 6530 psi | 50 mm/min; ISO 527 | |
| 47.0 MPa | 6820 psi | Type I, 50 mm/min; ASTM D638 | |
| Tensile Strength, Yield | 55.0 MPa | 7980 psi | 5 mm/min; ISO 527 |
| 55.0 MPa | 7980 psi | 50 mm/min; ISO 527 | |
| 57.0 MPa | 8270 psi | Type I, 50 mm/min; ASTM D638 | |
| Elongation at Break | >= 50 % | >= 50 % | 50 mm/min; ISO 527 |
| 100 % | 100 % | Type I, 50 mm/min; ASTM D638 | |
| 100 % | 100 % | 5 mm/min; ISO 527 | |
| Elongation at Yield | 4.0 % | 4.0 % | 50 mm/min; ISO 527 |
| 5.0 % | 5.0 % | Type I, 50 mm/min; ASTM D638 | |
| 5.0 % | 5.0 % | 5 mm/min; ISO 527 | |
| Tensile Modulus | 2.27 GPa | 329 ksi | 5 mm/min; ASTM D638 |
| 2.40 GPa | 348 ksi | 1 mm/min; ISO 527 | |
| Flexural Yield Strength | 80.0 MPa | 11600 psi | 2 mm/min; ISO 178 |
| 88.0 MPa | 12800 psi | 1.3 mm/min, 50 mm span; ASTM D790 | |
| Flexural Modulus | 2.30 GPa | 334 ksi | 1.3 mm/min, 50 mm span; ASTM D790 |
| 2.30 GPa | 334 ksi | 2 mm/min; ISO 178 | |
| Izod Impact, Notched | 5.80 J/cm | 10.9 ft-lb/in | ASTM D256 |
| 4.80 J/cm @Temperature -30.0 °C |
8.99 ft-lb/in @Temperature -22.0 °F |
ASTM D256 | |
| Izod Impact, Notched (ISO) | 50.0 kJ/m² | 23.8 ft-lb/in² | 80*10*3; ISO 180/1A |
| 30.0 kJ/m² @Temperature -30.0 °C |
14.3 ft-lb/in² @Temperature -22.0 °F |
80*10*3; ISO 180/1A | |
| Charpy Impact, Notched | 5.00 J/cm² | 23.8 ft-lb/in² | Edgew 80*10*3 sp=62mm; ISO 179/1eA |
| 3.00 J/cm² @Temperature -30.0 °C |
14.3 ft-lb/in² @Temperature -22.0 °F |
Edgew 80*10*3 sp=62mm; ISO 179/1eA | |
| Dart Drop, Total Energy | 54.0 J @Temperature 23.0 °C |
39.8 ft-lb @Temperature 73.4 °F |
ASTM D3763 |
| Taber Abrasion, mg/1000 Cycles | 63 | 63 | CS-17, 1 kg; SABIC Method |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 72.0 µm/m-°C @Temperature -40.0 - 40.0 °C |
40.0 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 |
| 80.0 µm/m-°C @Temperature 23.0 - 60.0 °C |
44.4 µin/in-°F @Temperature 73.4 - 140 °F |
ISO 11359-2 | |
| CTE, linear, Transverse to Flow | 72.0 µm/m-°C @Temperature -40.0 - 40.0 °C |
40.0 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 |
| 80.0 µm/m-°C @Temperature 23.0 - 60.0 °C |
44.4 µin/in-°F @Temperature 73.4 - 140 °F |
ISO 11359-2 | |
| Thermal Conductivity | 0.200 W/m-K | 1.39 BTU-in/hr-ft²-°F | ISO 8302 |
| Deflection Temperature at 0.46 MPa (66 psi) | 122 °C | 252 °F | Edgew 120*10*4 sp=100mm; ISO 75/Be |
| Deflection Temperature at 1.8 MPa (264 psi) | 102 °C | 216 °F | Edgew 120*10*4 sp=100mm; ISO 75/Ae |
| 112 °C @Thickness 3.20 mm |
234 °F @Thickness 0.126 in |
unannealed; ASTM D648 | |
| Vicat Softening Point | 126 °C | 259 °F | Rate B/50; ISO 306 |
| 128 °C | 262 °F | Rate B/120; ISO 306 | |
| 130 °C | 266 °F | Rate B/50; ASTM D1525 | |
| UL RTI, Electrical | 105 °C | 221 °F | UL 746B |
| UL RTI, Mechanical with Impact | 80.0 °C | 176 °F | UL 746B |
| UL RTI, Mechanical without Impact | 105 °C | 221 °F | UL 746B |
| Flammability, UL94 | HB @Thickness 1.20 mm |
HB @Thickness 0.0472 in |
UL 94 |
| HB @Thickness 3.00 mm |
HB @Thickness 0.118 in |
UL 94 | |
| Oxygen Index | 23 % | 23 % | ISO 4589 |
| Glow Wire Test | 650 °C @Thickness 1.00 mm |
1200 °F @Thickness 0.0394 in |
IEC 60695-2-12 |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Volume Resistivity | >= 1.00e+15 ohm-cm | >= 1.00e+15 ohm-cm | IEC 60093 |
| Surface Resistance | >= 1.00e+15 ohm | >= 1.00e+15 ohm | ROA; IEC 60093 |
| Dielectric Constant | 2.7 @Frequency 1.00e+6 Hz |
2.7 @Frequency 1.00e+6 Hz |
IEC 60250 |
| 2.8 @Frequency 50.0 - 60.0 Hz |
2.8 @Frequency 50.0 - 60.0 Hz |
IEC 60250 | |
| Dielectric Strength | 17.0 kV/mm @Thickness 3.20 mm |
432 kV/in @Thickness 0.126 in |
in oil; IEC 60243-1 |
| 25.0 kV/mm @Thickness 1.60 mm |
635 kV/in @Thickness 0.0630 in |
in oil; IEC 60243-1 | |
| 35.0 kV/mm @Thickness 0.800 mm |
889 kV/in @Thickness 0.0315 in |
in oil; IEC 60243-1 | |
| Dissipation Factor | 0.0020 @Frequency 50.0 - 60.0 Hz |
0.0020 @Frequency 50.0 - 60.0 Hz |
IEC 60250 |
| 0.0070 @Frequency 1.00e+6 Hz |
0.0070 @Frequency 1.00e+6 Hz |
IEC 60250 | |
| Comparative Tracking Index | 250 V | 250 V | IEC 60112 |
| Descriptive Properties | Value | Comments |
|---|---|---|
| Ball Pressure Test, 125°C +/- 2°C | PASSES | IEC 60695-10-2 |