Overview of materials for Polycarbonate, Molded

Category Polymer , Thermoplastic , Polycarbonate (PC) , Polycarbonate, Molded
Manufacturer
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Polycarbonate, Molded.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Polycarbonate, Molded". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 0.950 - 1.51 g/cc
0.0343 - 0.0546 lb/in³
Average value: 1.20 g/cc Grade Count:482
0.960 - 1.02 g/cc

@Temperature 280 - 330 °C
0.0347 - 0.0368 lb/in³

@Temperature 536 - 626 °F
Average value: 1.01 g/cc Grade Count:43
Water Absorption 0.0150 - 0.400 %
0.0150 - 0.400 %
Average value: 0.237 % Grade Count:249
Moisture Absorption at Equilibrium 0.120 - 0.350 %
0.120 - 0.350 %
Average value: 0.147 % Grade Count:114
Water Absorption at Saturation 0.300 - 0.400 %
0.300 - 0.400 %
Average value: 0.313 % Grade Count:54
Water Vapor Transmission 15.0 g/m²/day
0.966 g/100 in²/day
Average value: 15.0 g/m²/day Grade Count:19
Oxygen Transmission 65.0 - 80.0 cc-mm/m²-24hr-atm
165 - 203 cc-mil/100 in²-24hr-atm
Average value: 71.4 cc-mm/m²-24hr-atm Grade Count:20
Nitrogen Transmission 12.0 - 16.0 cc-mm/m²-24hr-atm
30.5 - 40.6 cc-mil/100 in²-24hr-atm
Average value: 13.5 cc-mm/m²-24hr-atm Grade Count:20
Carbon Dioxide Transmission 380 - 480 cc-mm/m²-24hr-atm
965 - 1220 cc-mil/100 in²-24hr-atm
Average value: 429 cc-mm/m²-24hr-atm Grade Count:20
Viscosity Test 42.0 - 68.0 cm³/g
42.0 - 68.0 cm³/g
Average value: 54.7 cm³/g Grade Count:39
Maximum Moisture Content 0.0200
0.0200
Average value: 0.0200 Grade Count:30
Linear Mold Shrinkage 0.00100 - 0.0100 cm/cm
0.00100 - 0.0100 in/in
Average value: 0.00624 cm/cm Grade Count:373
Linear Mold Shrinkage, Transverse 0.00400 - 0.00800 cm/cm
0.00400 - 0.00800 in/in
Average value: 0.00677 cm/cm Grade Count:95
Melt Flow 1.00 - 120 g/10 min
1.00 - 120 g/10 min
Average value: 16.1 g/10 min Grade Count:403
Mechanical Properties Metric English Comments
Hardness, Rockwell M 65.0 - 122
65.0 - 122
Average value: 72.3 Grade Count:101
Hardness, Rockwell R 72.0 - 123
72.0 - 123
Average value: 119 Grade Count:120
Ball Indentation Hardness 111 - 118 MPa
16100 - 17100 psi
Average value: 115 MPa Grade Count:35
Tensile Strength, Ultimate 46.1 - 93.1 MPa
6690 - 13500 psi
Average value: 64.5 MPa Grade Count:208
23.0 - 51.0 MPa

@Temperature 60.0 - 120 °C
3340 - 7400 psi

@Temperature 140 - 248 °F
Average value: 38.1 MPa Grade Count:4
Tensile Strength, Yield 37.0 - 154 MPa
5370 - 22300 psi
Average value: 63.3 MPa Grade Count:371
Elongation at Break 3.00 - 233 %
3.00 - 233 %
Average value: 82.7 % Grade Count:378
70.0 - 70.0 %

@Temperature 60.0 - 120 °C
70.0 - 70.0 %

@Temperature 140 - 248 °F
Average value: 90.0 % Grade Count:1
Elongation at Yield 5.00 - 110 %
5.00 - 110 %
Average value: 8.03 % Grade Count:219
2.50 - 4.00 %

@Temperature 60.0 - 120 °C
2.50 - 4.00 %

@Temperature 140 - 248 °F
Average value: 3.17 % Grade Count:1
Modulus of Elasticity 1.80 - 3.00 GPa
261 - 435 ksi
Average value: 2.34 GPa Grade Count:243
1.60 - 2.10 GPa

@Temperature 60.0 - 120 °C
232 - 305 ksi

@Temperature 140 - 248 °F
Average value: 1.83 GPa Grade Count:1
Flexural Yield Strength 27.6 - 205 MPa
4000 - 29700 psi
Average value: 90.5 MPa Grade Count:340
Flexural Modulus 0.228 - 10.0 GPa
33.0 - 1450 ksi
Average value: 2.35 GPa Grade Count:391
1.70 - 2.20 GPa

@Temperature 60.0 - 120 °C
247 - 319 ksi

@Temperature 140 - 248 °F
Average value: 1.88 GPa Grade Count:3
Compressive Yield Strength 76.0 - 86.2 MPa
11000 - 12500 psi
Average value: 82.8 MPa Grade Count:9
Izod Impact, Notched 0.392 J/cm - NB
0.735 ft-lb/in - NB
Average value: 6.42 J/cm Grade Count:272
1.00 - 5.339 J/cm

@Temperature -40.0 - 0.000 °C
1.87 - 10.00 ft-lb/in

@Temperature -40.0 - 32.0 °F
Average value: 3.16 J/cm Grade Count:9
2.1356 - 2.1356 J/cm

@Temperature -40.0 - -30.0 °C
4.0009 - 4.0009 ft-lb/in

@Temperature -40.0 - -22.0 °F
Average value: 3.16 J/cm Grade Count:3
2.1356 - 2.1356 J/cm

@Thickness 3.17 - 3.20 mm
4.0009 - 4.0009 ft-lb/in

@Thickness 0.125 - 0.126 in
Average value: 3.16 J/cm Grade Count:3
Izod Impact, Unnotched 7.35 - 5340 J/cm
13.8 - 10000 ft-lb/in
Average value: 12.2 J/cm Grade Count:46
Izod Impact, Notched (ISO) 8.00 - 90.0 kJ/m²
3.81 - 42.8 ft-lb/in²
Average value: 71.6 kJ/m² Grade Count:85
60.0 - 60.0 kJ/m²

@Temperature -20.0 - -20.0 °C
28.6 - 28.6 ft-lb/in²

@Temperature -4.00 - -4.00 °F
Average value: 15.1 kJ/m² Grade Count:3
12.0 - 16.0 kJ/m²

@Temperature -30.0 - -30.0 °C
5.71 - 7.61 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 15.1 kJ/m² Grade Count:36
12.0 - 16.0 kJ/m²

@Thickness 3.20 - 3.20 mm
5.71 - 7.61 ft-lb/in²

@Thickness 0.126 - 0.126 in
Average value: 15.1 kJ/m² Grade Count:36
Charpy Impact Unnotched 22.0 J/cm² - NB
105 ft-lb/in² - NB
Average value: 28.4 J/cm² Grade Count:133
25.0 J/cm² - NB

@Temperature -60.0 - -20.0 °C
119 ft-lb/in² - NB

@Temperature -76.0 - -4.00 °F
Average value: 29.3 J/cm² Grade Count:107
Charpy Impact, Notched 0.600 - 8.90 J/cm²
2.86 - 42.4 ft-lb/in²
Average value: 5.14 J/cm² Grade Count:67
0.600 - 1.00 J/cm²

@Temperature -30.0 - -20.0 °C
2.86 - 4.76 ft-lb/in²

@Temperature -22.0 - -4.00 °F
Average value: 1.34 J/cm² Grade Count:15
1.20 - 1.80 J/cm²

@Temperature -30.0 - -30.0 °C
5.71 - 8.57 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 1.34 J/cm² Grade Count:33
1.20 - 1.80 J/cm²

@Thickness 3.00 - 3.00 mm
5.71 - 8.57 ft-lb/in²

@Thickness 0.118 - 0.118 in
Average value: 1.34 J/cm² Grade Count:33
Gardner Impact 36.2 - 169 J
26.7 - 125 ft-lb
Average value: 39.7 J Grade Count:38
>= 36.1552 J

@Temperature -30.0 - -18.0 °C
>= 26.6667 ft-lb

@Temperature -22.0 - -0.400 °F
Average value: 36.2 J Grade Count:5
Tensile Impact Strength 546 - 580 kJ/m²
260 - 276 ft-lb/in²
Average value: 572 kJ/m² Grade Count:4
Dart Drop, Total Energy 16.0 J
11.8 ft-lb
Average value: 16.0 J Grade Count:3
11.0 - 16.0 J

@Temperature -30.0 - -30.0 °C
8.11 - 11.8 ft-lb

@Temperature -22.0 - -22.0 °F
Average value: 14.3 J Grade Count:3
Falling Dart Impact 53.8 - 1300 J
39.7 - 960 ft-lb
Average value: 774 J Grade Count:7
75.9 - 75.9 J

@Temperature -40.0 - -40.0 °C
56.0 - 56.0 ft-lb

@Temperature -40.0 - -40.0 °F
Average value: 75.9 J Grade Count:1
Users viewing this material also viewed the following: