Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Polypropylene with 40% Talc Filler". Specific grades with primary filler content between 35% and 44% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.10 - 1.56 g/cc
0.0397 - 0.0564 lb/in³
Average value: 1.24 g/cc Grade Count:177
Filler Content 30.0 - 40.0 %
30.0 - 40.0 %
Average value: 39.7 % Grade Count:83
Water Absorption 0.0200 - 0.0400 %
0.0200 - 0.0400 %
Average value: 0.0277 % Grade Count:13
Linear Mold Shrinkage 0.00300 - 0.0200 cm/cm
0.00300 - 0.0200 in/in
Average value: 0.00955 cm/cm Grade Count:136
Linear Mold Shrinkage, Transverse 0.00560 - 0.0165 cm/cm
0.00560 - 0.0165 in/in
Average value: 0.0126 cm/cm Grade Count:18
Melt Flow 1.00 - 30.0 g/10 min
1.00 - 30.0 g/10 min
Average value: 10.1 g/10 min Grade Count:156
Ash 34.0 - 45.0 %
34.0 - 45.0 %
Average value: 39.9 % Grade Count:19
37.0 - 63.0 %

@Temperature 600 - 600 °C
37.0 - 63.0 %

@Temperature 1110 - 1110 °F
Average value: 42.0 % Grade Count:5
Mechanical Properties Metric English Comments
Hardness, Rockwell M 50.0 - 100
50.0 - 100
Average value: 64.5 Grade Count:6
Hardness, Rockwell R 42.0 - 102
42.0 - 102
Average value: 84.8 Grade Count:34
Hardness, Shore D 65.0 - 84.0
65.0 - 84.0
Average value: 72.8 Grade Count:20
Tensile Strength, Ultimate 13.0 - 50.0 MPa
1890 - 7250 psi
Average value: 27.6 MPa Grade Count:116
7.00 - 18.0 MPa

@Temperature 60.0 - 120 °C
1020 - 2610 psi

@Temperature 140 - 248 °F
Average value: 12.3 MPa Grade Count:1
Tensile Strength, Yield 13.8 - 60.0 MPa
2000 - 8700 psi
Average value: 29.2 MPa Grade Count:76
Elongation at Break 3.00 - 70.0 %
3.00 - 70.0 %
Average value: 10.2 % Grade Count:77
Elongation at Yield 2.00 - 25.0 %
2.00 - 25.0 %
Average value: 5.20 % Grade Count:74
Modulus of Elasticity 1.40 - 5.17 GPa
203 - 750 ksi
Average value: 3.21 GPa Grade Count:45
Flexural Yield Strength 20.0 - 75.0 MPa
2900 - 10900 psi
Average value: 48.5 MPa Grade Count:100
Flexural Modulus 1.50 - 5.70 GPa
218 - 827 ksi
Average value: 3.21 GPa Grade Count:175
0.450 - 1.40 GPa

@Temperature 60.0 - 120 °C
65.3 - 203 ksi

@Temperature 140 - 248 °F
Average value: 0.883 GPa Grade Count:1
Compressive Yield Strength 51.7 MPa
7500 psi
Average value: 51.7 MPa Grade Count:3
Izod Impact, Notched 0.200 - 1.33 J/cm
0.375 - 2.50 ft-lb/in
Average value: 0.377 J/cm Grade Count:106
0.200 - 0.300 J/cm

@Temperature -40.0 - -20.0 °C
0.375 - 0.562 ft-lb/in

@Temperature -40.0 - -4.00 °F
Average value: 0.267 J/cm Grade Count:2
Izod Impact, Unnotched 1.39 - 9.08 J/cm
2.60 - 17.0 ft-lb/in
Average value: 2.95 J/cm Grade Count:33
Izod Impact, Notched (ISO) 2.00 - 12.0 kJ/m²
0.952 - 5.71 ft-lb/in²
Average value: 4.05 kJ/m² Grade Count:14
1.60 - 3.00 kJ/m²

@Temperature -40.0 - -20.0 °C
0.761 - 1.43 ft-lb/in²

@Temperature -40.0 - -4.00 °F
Average value: 2.18 kJ/m² Grade Count:9
Charpy Impact Unnotched 1.70 - 1000 J/cm²
8.09 - 4760 ft-lb/in²
Average value: 4.44 J/cm² Grade Count:23
0.900 - 6.40 J/cm²

@Temperature -40.0 - -20.0 °C
4.28 - 30.5 ft-lb/in²

@Temperature -40.0 - -4.00 °F
Average value: 1.77 J/cm² Grade Count:22
Charpy Impact, Notched 0.200 - 2.70 J/cm²
0.952 - 12.8 ft-lb/in²
Average value: 0.477 J/cm² Grade Count:59
0.100 - 0.600 J/cm²

@Temperature -40.0 - -20.0 °C
0.476 - 2.86 ft-lb/in²

@Temperature -40.0 - -4.00 °F
Average value: 0.193 J/cm² Grade Count:46
Gardner Impact 0.565 - 13.6 J
0.417 - 10.0 ft-lb
Average value: 2.05 J Grade Count:32
1.35582 - 1.35582 J

@Temperature -30.0 - -5.56 °C
1.00000 - 1.00000 ft-lb

@Temperature -22.0 - 22.0 °F
Average value: 3.11 J Grade Count:2
4.86 - 4.86 J

@Temperature -23.0 - -23.0 °C
3.58 - 3.58 ft-lb

@Temperature -9.40 - -9.40 °F
Average value: 3.11 J Grade Count:1
4.86 - 4.86 J

@Thickness 3.18 - 3.18 mm
3.58 - 3.58 ft-lb

@Thickness 0.125 - 0.125 in
Average value: 3.11 J Grade Count:1
Thermal Properties Metric English Comments
CTE, linear 41.4 - 172 µm/m-°C
23.0 - 95.6 µin/in-°F
Average value: 67.7 µm/m-°C Grade Count:11
Thermal Conductivity 0.317 W/m-K
2.20 BTU-in/hr-ft²-°F
Average value: 0.317 W/m-K Grade Count:3
Melting Point 150 - 182 °C
302 - 360 °F
Average value: 159 °C Grade Count:19
Deflection Temperature at 0.46 MPa (66 psi) 94.0 - 150 °C
201 - 302 °F
Average value: 128 °C Grade Count:140
Deflection Temperature at 1.8 MPa (264 psi) 56.0 - 142 °C
133 - 287 °F
Average value: 81.1 °C Grade Count:143
Vicat Softening Point 54.0 - 165 °C
129 - 329 °F
Average value: 119 °C Grade Count:71
Flammability, UL94 HB
HB
Grade Count:77
Oxygen Index 21.0 - 22.0 %
21.0 - 22.0 %
Average value: 21.2 % Grade Count:6
Glow Wire Test 650 - 750 °C
1200 - 1380 °F
Average value: 742 °C Grade Count:47
Optical Properties Metric English Comments
Gloss 20.0 - 40.0 %
20.0 - 40.0 %
Average value: 32.3 % Grade Count:3
Electrical Properties Metric English Comments
Electrical Resistivity 1.00e+15 - 1.00e+16 ohm-cm
1.00e+15 - 1.00e+16 ohm-cm
Average value: 8.50e+15 ohm-cm Grade Count:6
Dielectric Constant 2.60 - 4.80
2.60 - 4.80
Average value: 3.15 Grade Count:4
Dielectric Strength 19.7 - 24.0 kV/mm
500 - 610 kV/in
Average value: 21.4 kV/mm Grade Count:7
Dissipation Factor 0.00800
0.00800
Average value: 0.00800 Grade Count:3
Arc Resistance 120 sec
120 sec
Average value: 120 sec Grade Count:3
Comparative Tracking Index 600 V
600 V
Average value: 600 V Grade Count:5
Processing Properties Metric English Comments
Processing Temperature 193 - 227 °C
380 - 440 °F
Average value: 210 °C Grade Count:5
Nozzle Temperature 200 - 238 °C
392 - 460 °F
Average value: 226 °C Grade Count:28
Melt Temperature 170 - 279 °C
338 - 534 °F
Average value: 224 °C Grade Count:92
Mold Temperature 18.0 - 80.0 °C
64.4 - 176 °F
Average value: 51.0 °C Grade Count:95
Drying Temperature 65.6 - 104 °C
150 - 219 °F
Average value: 76.8 °C Grade Count:77
Users viewing this material also viewed the following: