Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Epoxy, Cast, Aluminum Filled". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 0.959 - 3.12 g/cc
0.0346 - 0.113 lb/in³
Average value: 1.94 g/cc Grade Count:17
Water Absorption 0.0300 - 0.450 %
0.0300 - 0.450 %
Average value: 0.162 % Grade Count:5
Porosity 15.0 - 16.0 %
15.0 - 16.0 %
Average value: 15.7 % Grade Count:3
Viscosity 3000 - 160000 cP
3000 - 160000 cP
Average value: 42400 cP Grade Count:7
Pore Size 12.7 - 15.2 microns
0.500 - 0.600 mil
Average value: 13.5 microns Grade Count:3
Linear Mold Shrinkage 0.00100 - 0.00400 cm/cm
0.00100 - 0.00400 in/in
Average value: 0.00240 cm/cm Grade Count:5
Mechanical Properties Metric English Comments
Hardness, Shore D 81.0 - 95.0
81.0 - 95.0
Average value: 86.5 Grade Count:22
Tensile Strength, Ultimate 0.159 - 59.6 MPa
23.0 - 8650 psi
Average value: 26.7 MPa Grade Count:20
Tensile Strength, Yield 6.89 - 20.7 MPa
1000 - 3000 psi
Average value: 16.5 MPa Grade Count:5
Elongation at Break 0.000 - 130 %
0.000 - 130 %
Average value: 19.6 % Grade Count:7
Modulus of Elasticity 4.14 - 8.27 GPa
600 - 1200 ksi
Average value: 6.18 GPa Grade Count:6
Flexural Yield Strength 3.45 - 56.0 MPa
500 - 8130 psi
Average value: 31.0 MPa Grade Count:16
Flexural Modulus 9.00 - 10.8 GPa
1310 - 1570 ksi
Average value: 9.67 GPa Grade Count:3
Compressive Yield Strength 41.4 - 89.6 MPa
6000 - 13000 psi
Average value: 73.1 MPa Grade Count:18
Compressive Modulus 3.45 - 5.17 GPa
500 - 750 ksi
Average value: 4.41 GPa Grade Count:5
Shear Strength 13.8 - 31.0 MPa
2000 - 4500 psi
Average value: 20.6 MPa Grade Count:17
1.70 - 31.0 MPa

@Temperature -55.0 - 177 °C
247 - 4500 psi

@Temperature -67.0 - 351 °F
Average value: 14.2 MPa Grade Count:5
Adhesive Bond Strength 6.89 - 42.1 MPa
1000 - 6100 psi
Average value: 19.1 MPa Grade Count:7
19.3053 - 27.9238 MPa

@Temperature -54.4 - 82.2 °C
2800.00 - 4050.01 psi

@Temperature -66.0 - 180 °F
Average value: 23.6 MPa Grade Count:1
Thermal Properties Metric English Comments
CTE, linear 31.0 - 53.0 µm/m-°C
17.2 - 29.4 µin/in-°F
Average value: 41.3 µm/m-°C Grade Count:7
30.06 - 111 µm/m-°C

@Temperature 25.0 - 125 °C
16.70 - 61.7 µin/in-°F

@Temperature 77.0 - 257 °F
Average value: 76.9 µm/m-°C Grade Count:8
Thermal Conductivity 0.724 - 1.28 W/m-K
5.02 - 8.88 BTU-in/hr-ft²-°F
Average value: 1.08 W/m-K Grade Count:6
19.0 - 20.5 W/m-K

@Temperature 100 - 100 °C
132 - 142 BTU-in/hr-ft²-°F

@Temperature 212 - 212 °F
Average value: 19.5 W/m-K Grade Count:3
Maximum Service Temperature, Air 108 - 210 °C
226 - 410 °F
Average value: 145 °C Grade Count:10
Minimum Service Temperature, Air -60.0 - -20.0 °C
-76.0 - -4.00 °F
Average value: -46.0 °C Grade Count:5
Glass Transition Temp, Tg 55.0 - 132 °C
131 - 270 °F
Average value: 92.8 °C Grade Count:6
Electrical Properties Metric English Comments
Electrical Resistivity 1.00e+15 ohm-cm
1.00e+15 ohm-cm
Average value: 1.00e+15 ohm-cm Grade Count:5
Dielectric Constant 4.90 - 21.4
4.90 - 21.4
Average value: 7.90 Grade Count:6
Dielectric Strength 3.94 - 15.7 kV/mm
100 - 400 kV/in
Average value: 13.1 kV/mm Grade Count:6
Processing Properties Metric English Comments
Processing Temperature 21.1 - 260 °C
70.0 - 500 °F
Average value: 133 °C Grade Count:7
Cure Time 480 - 1440 min
8.00 - 24.0 hour
Average value: 880 min Grade Count:3
30.0 - 720 min

@Temperature 45.0 - 150 °C
0.500 - 12.0 hour

@Temperature 113 - 302 °F
Average value: 284 min Grade Count:11
Pot Life 30.0 - 100000 min
30.0 - 100000 min
Average value: 5460 min Grade Count:19