Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Nylon 66, PTFE Filled

Category Polymer , Thermoplastic , Nylon , Nylon 66 , Nylon 66, PTFE Filled
Manufacturer
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Nylon 66, PTFE Filled.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Nylon 66, PTFE Filled". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.11 - 1.60 g/cc
0.0401 - 0.0578 lb/in³
Average value: 1.30 g/cc Grade Count:112
Filler Content 10.0 - 30.0 %
10.0 - 30.0 %
Average value: 18.3 % Grade Count:3
Water Absorption 0.300 - 8.50 %
0.300 - 8.50 %
Average value: 0.899 % Grade Count:77
Moisture Absorption at Equilibrium 0.300 - 2.80 %
0.300 - 2.80 %
Average value: 1.24 % Grade Count:5
Water Absorption at Saturation 5.00 - 6.00 %
5.00 - 6.00 %
Average value: 5.50 % Grade Count:3
Additive Loading 5.00 - 15.0 %
5.00 - 15.0 %
Average value: 10.0 % Grade Count:3
Linear Mold Shrinkage 0.00200 - 0.0400 cm/cm
0.00200 - 0.0400 in/in
Average value: 0.0160 cm/cm Grade Count:109
Linear Mold Shrinkage, Transverse 0.0100 - 0.0400 cm/cm
0.0100 - 0.0400 in/in
Average value: 0.0188 cm/cm Grade Count:10
Melt Flow 10.0 - 14.3 g/10 min
10.0 - 14.3 g/10 min
Average value: 12.4 g/10 min Grade Count:3
Mechanical Properties Metric English Comments
Hardness, Rockwell R 90.0 - 122
90.0 - 122
Average value: 108 Grade Count:40
Tensile Strength, Ultimate 35.9 - 170 MPa
5200 - 24700 psi
Average value: 62.9 MPa Grade Count:84
Tensile Strength, Yield 40.7 - 181 MPa
5900 - 26200 psi
Average value: 114 MPa Grade Count:35
131 - 131 MPa

@Temperature 93.3 - 93.3 °C
19000 - 19000 psi

@Temperature 200 - 200 °F
Average value: 131 MPa Grade Count:1
Elongation at Break 2.00 - 40.0 %
2.00 - 40.0 %
Average value: 6.73 % Grade Count:92
Elongation at Yield 2.00 - 40.0 %
2.00 - 40.0 %
Average value: 7.26 % Grade Count:26
Modulus of Elasticity 1.65 - 10.0 GPa
240 - 1450 ksi
Average value: 2.80 GPa Grade Count:69
Flexural Yield Strength 50.0 - 303 MPa
7250 - 44000 psi
Average value: 115 MPa Grade Count:108
Flexural Modulus 1.38 - 11.0 GPa
200 - 1600 ksi
Average value: 3.70 GPa Grade Count:107
8.96318 - 8.96318 GPa

@Temperature 93.3 - 93.3 °C
1300.02 - 1300.02 ksi

@Temperature 200 - 200 °F
Average value: 8.96 GPa Grade Count:1
Compressive Yield Strength 30.3 - 68.9 MPa
4400 - 10000 psi
Average value: 46.5 MPa Grade Count:10
Izod Impact, Notched 0.210 - 2.67 J/cm
0.393 - 5.00 ft-lb/in
Average value: 0.768 J/cm Grade Count:93
Izod Impact, Unnotched 1.60 J/cm - NB
3.00 ft-lb/in - NB
Average value: 8.75 J/cm Grade Count:58
Izod Impact, Notched (ISO) 2.00 - 13.0 kJ/m²
0.952 - 6.19 ft-lb/in²
Average value: 4.38 kJ/m² Grade Count:9
11.0 - 11.0 kJ/m²

@Temperature -30.0 - -30.0 °C
5.23 - 5.23 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 11.0 kJ/m² Grade Count:1
Izod Impact, Unnotched (ISO) 10.0 - 80.0 kJ/m²
4.76 - 38.1 ft-lb/in²
Average value: 34.7 kJ/m² Grade Count:9
70.0 - 70.0 kJ/m²

@Temperature -30.0 - -30.0 °C
33.3 - 33.3 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 70.0 kJ/m² Grade Count:1
Charpy Impact Unnotched 2.50 J/cm² - NB
11.9 ft-lb/in² - NB
Average value: 6.52 J/cm² Grade Count:18
3.20 J/cm² - NB

@Temperature -40.0 - -30.0 °C
15.2 ft-lb/in² - NB

@Temperature -40.0 - -22.0 °F
Average value: 5.13 J/cm² Grade Count:12
Charpy Impact, Notched 0.280 - 1.40 J/cm²
1.33 - 6.66 ft-lb/in²
Average value: 0.715 J/cm² Grade Count:11
0.400 - 0.800 J/cm²

@Temperature -40.0 - -30.0 °C
1.90 - 3.81 ft-lb/in²

@Temperature -40.0 - -22.0 °F
Average value: 0.625 J/cm² Grade Count:3
Falling Dart Impact 0.570 - 4.10 J
0.420 - 3.02 ft-lb
Average value: 2.55 J Grade Count:5
Coefficient of Friction 0.0700 - 0.500
0.0700 - 0.500
Average value: 0.207 Grade Count:34
Coefficient of Friction, Static 0.0600 - 0.390
0.0600 - 0.390
Average value: 0.162 Grade Count:34
K (wear) Factor 6.20 - 359 x 10-8 mm³/N-M
3.08 - 178 x 10-10 in³-min/ft-lb-hr
Average value: 67.2 x 10<sup>-8</sup> mm³/N-M Grade Count:22
Limiting Pressure Velocity 0.333 - 0.701 MPa-m/sec
9500 - 20000 psi-ft/min
Average value: 0.587 MPa-m/sec Grade Count:11
Thermal Properties Metric English Comments
CTE, linear 18.0 - 82.8 µm/m-°C
10.0 - 46.0 µin/in-°F
Average value: 53.1 µm/m-°C Grade Count:50
Thermal Conductivity 0.230 - 0.418 W/m-K
1.60 - 2.90 BTU-in/hr-ft²-°F
Average value: 0.255 W/m-K Grade Count:16
Melting Point 254 - 275 °C
490 - 527 °F
Average value: 259 °C Grade Count:11
Maximum Service Temperature, Air 90.0 - 160 °C
194 - 320 °F
Average value: 126 °C Grade Count:17
Deflection Temperature at 0.46 MPa (66 psi) 155 - 260 °C
311 - 500 °F
Average value: 223 °C Grade Count:50
Deflection Temperature at 1.8 MPa (264 psi) 63.0 - 260 °C
145 - 500 °F
Average value: 129 °C Grade Count:100
Vicat Softening Point 200 - 250 °C
392 - 482 °F
Average value: 234 °C Grade Count:15
Flammability, UL94 HB - V-0
HB - V-0
Grade Count:67
Electrical Properties Metric English Comments
Electrical Resistivity 1.00e+14 - 1.00e+16 ohm-cm
1.00e+14 - 1.00e+16 ohm-cm
Average value: 1.52e+15 ohm-cm Grade Count:64
Surface Resistance 1.00e+9 - 1.00e+13 ohm
1.00e+9 - 1.00e+13 ohm
Average value: 1.54e+12 ohm Grade Count:13
Insulation Resistance 1.00e+9 - 1.00e+12 ohm
1.00e+9 - 1.00e+12 ohm
Average value: 8.42e+11 ohm Grade Count:12
Dielectric Constant 3.60 - 3.70
3.60 - 3.70
Average value: 3.63 Grade Count:6
Dielectric Strength 17.3 - 23.6 kV/mm
440 - 600 kV/in
Average value: 19.9 kV/mm Grade Count:33
Dissipation Factor 0.0100 - 0.0200
0.0100 - 0.0200
Average value: 0.0161 Grade Count:9
Comparative Tracking Index 550 - 600 V
550 - 600 V
Average value: 583 V Grade Count:3
Processing Properties Metric English Comments
Processing Temperature 270 - 300 °C
518 - 572 °F
Average value: 287 °C Grade Count:34
Nozzle Temperature 280 - 300 °C
536 - 572 °F
Average value: 290 °C Grade Count:14
Melt Temperature 260 - 310 °C
500 - 590 °F
Average value: 294 °C Grade Count:49
Mold Temperature 49.0 - 121 °C
120 - 250 °F
Average value: 90.2 °C Grade Count:66
Drying Temperature 75.0 - 105 °C
167 - 221 °F
Average value: 85.0 °C Grade Count:49
Users viewing this material also viewed the following: